Method for measuring trace iron content in lithium carbonate for battery
Through the ICP-MS analysis method, combined with dilute nitric acid dissolution and scandium internal standard elimination of interference, the rapid and accurate determination of trace iron in lithium carbonate is achieved, which solves the problems of cumbersome operation and insufficient detection limit of the existing method and meets the needs of high-purity carbonic acid. Lithium testing requirements for iron content.
Patent Information
- Application Number
- CN202411056944.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-29
AI Technical Summary
The existing methods for determining the iron content in lithium carbonate are cumbersome to operate, use many reagents, and cannot meet the lower detection limit requirements of impurity elements in modern production. They cannot meet the detection requirements for iron content in high-purity lithium carbonate.
Using the ICP-MS analysis method, the lithium carbonate sample is dissolved with dilute nitric acid, and the scandium internal standard standard solution is added online to eliminate the interference of the lithium matrix. The dynamic reaction cell mode is used to perform a gas-phase chemical reaction with ammonia to generate non-interfering substances, which are inductively coupled Trace iron content determined on a plasma mass spectrometer.
It achieves fast, accurate, and easy-to-operate trace iron content determination, with a lower detection limit of 0.00001% and a relative standard deviation of less than 20%. It meets the detection requirements for iron content in high-purity lithium carbonate and has a low detection limit, fast analysis speed, and accuracy. Practical features.
Smart Images

Figure SMS_2 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal impurity element testing and analysis in the battery material industry, and in particular relates to a method for determining trace iron content in lithium carbonate for batteries. Background Art
[0002] As the country vigorously develops new energy technologies, lithium-ion batteries have been widely used due to their advantages such as light weight, large capacity, high voltage and no memory effect. Positive electrode materials, negative electrode materials, diaphragms and electrolytes are the four major components of lithium-ion batteries, of which positive electrode materials account for more than 40% of the total cost of lithium-ion batteries. Lithium carbonate is a key raw material for the preparation of lithium-ion positive electrode materials. It was once defined as "white oil" and has therefore attracted much attention in the upstream industries of new energy vehicles and power batteries.
[0003] Lithium carbonate for batteries is the core raw material in the production process of lithium ions. It is mainly used for positive electrode materials of lithium iron phosphate, lithium cobalt oxide and some ternary lithium. Its quality directly affects production safety, electrochemical performance of batteries, and safety of use. 3+ If the content is too high, it will seriously affect the safety performance of lithium batteries, so accurate determination of its impurities is of great significance.
[0004] Inductively coupled plasma mass spectrometer (ICP-MS) is an analytical instrument that combines ICP technology with mass spectrometry. It can simultaneously determine dozens of trace inorganic elements. Compared with traditional chemical methods and inductively coupled plasma spectrometers (ICP-AES), its detection limit is about 3 orders of magnitude lower. In addition, modern ICP-MS uses dynamic reaction cell (DRC) technology to chemically react NH3, CH4 and other gases with polyatomic ions, which can reduce their interference intensity by 7 orders of magnitude and remove 40 Ar 16 O to Fe 56 interference.
[0005] At present, the determination of iron content in lithium carbonate in China adopts the o-phenanthroline spectrophotometry (GB / T 11064.7-2013), that is, iron (III) is reduced to iron (II) with ascorbic acid, and iron (II) forms an orange-red complex with o-phenanthroline in an acetate buffer medium of pH 3.5, and the absorbance is measured at 510nm by a spectrophotometer to calculate the iron content in the sample. The determination range of this method is 0.00030% to 0.030%, and the determination operation is cumbersome, the reagents used are many, and it cannot meet the requirements of modern production for the lower limit of detection of impurity elements. Traditionally, lithium carbonate with higher purity is used in the manufacture of lithium cobalt oxide. The control limit of iron in 99.999% lithium carbonate is 0.00008%, the control limit of iron in 99.995% lithium carbonate is 0.0001%, and the control limit of iron in 99.99% lithium carbonate is 0.0003%. The lower limit of detection of colorimetry cannot meet the iron detection requirements of 4N and above levels. Summary of the invention
[0006] (1) Technical problem to be solved: In view of the fact that the existing determination methods are cumbersome to operate, use many reagents and cannot meet the requirements of modern production for the lower limit of detection of impurity elements, the present invention provides an accurate, rapid and easy-to-operate ICP-MS analysis method for trace iron in lithium carbonate, which solves the problem of determining the trace iron content in lithium carbonate for batteries and fills the gap in detection standards.
[0007] (2) The technical solution adopted by the present invention is as follows: A method for determining the trace iron content in lithium carbonate for batteries, based on which a lithium carbonate sample is dissolved in dilute nitric acid to a fixed volume, a scandium internal standard solution is added online to eliminate the interference of the lithium matrix, a dynamic reaction cell (DRC) mode is selected, ammonia is used as a reaction gas, a gas phase chemical reaction is produced with the interfering ions to generate non-interfering substances with other mass numbers, and the substances are determined on an inductively coupled plasma mass spectrometer, wherein the steps are as follows:
[0008] 1. Sample processing:
[0009] Weigh 0.2000g of lithium carbonate sample into a 200ml beaker, add first-grade water to completely soak the sample, slowly titrate 5mL of dilute nitric acid (1+1), cover with a watch glass, place the beaker on a hot plate and heat it to a small volume at low temperature, remove the beaker and cool it to room temperature, then transfer the solution in the beaker into a 100mL volumetric flask, dilute to the scale with first-grade water, mix well, and obtain a sample solution.
[0010] 2. Reagent blank test:
[0011] Add 5mL of dilute nitric acid (1+1) to a 200mL beaker, cover with a watch glass, place the beaker on a hot plate and heat to a small volume at low temperature, remove the beaker and cool to room temperature, rinse the beaker wall and watch glass with a wash bottle filled with first-grade water, continue to boil on the hot plate, remove the beaker and cool to room temperature, transfer the solution in the beaker to a 100mL volumetric flask, dilute to the scale with first-grade water, mix well, and obtain a blank sample solution.
[0012] 3. Configuration of standard series solutions
[0013] Standard storage solution: Iron and scandium, use valid, certified single-element standard storage solution with a mass concentration of 1000 μg / mL.
[0014] Iron standard solution A: Pipette 1.00 mL of the iron standard stock solution into a 100 mL volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix. This solution contains 10 μg of iron per mL.
[0015] Iron standard solution B: Pipette 1.00 mL of iron standard solution A into a 100 mL volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix well. This solution contains 100 μg of iron in 1 L.
[0016] Scandium internal standard solution: dilute the scandium standard storage solution step by step, and each liter of the diluted solution contains 10 μg of scandium. The medium is nitric acid (2+98).
[0017] 4. Draw the working curve: Pipette 0mL, 0.50mL, 1.00mL, 5.00mL, 10.00mL, 20.00mL, and 50.00mL of 100μg / L iron standard solution B into a set of 100mL volumetric flasks, add 2mL of concentrated nitric acid, dilute to the scale with first-grade water, and mix well. This standard solution contains 0μg, 0.5μg, 1.0μg, 5.0μg, 10.0μg, 20.0μg, and 50.0μg of iron per liter.
[0018] An inductively coupled plasma mass spectrometer was selected, and the measurement parameters were as follows: high frequency generator power 1300w, cooling gas 18.0L / min, auxiliary gas 1.2L / min, nebulizer gas 0.82L / min, measurement mode was pulse, and the analysis mass-to-charge ratio was 56Fe, on an inductively coupled plasma mass spectrometer, after the instrument runs stably, the working curve method and the online addition of scandium internal standard solution are used, the dynamic reaction cell (DRC) mode is selected, ammonia is used as the reaction gas, and a gas phase chemical reaction is produced with the interfering ions to generate non-interfering substances of other mass numbers, which are measured on the inductively coupled plasma mass spectrometer. The series of standard solutions are measured, and the instrument automatically draws the working curve. The correlation coefficient of the working curve of each element should be above 0.999, otherwise it is necessary to re-standardize or re-configure the series of standard solutions for standardization.
[0019] 5. Sample measurement: On the inductively coupled plasma mass spectrometer, after the instrument runs stably, under the same conditions as 4), use the working curve method and the method of adding the scandium internal standard solution online to measure the test solution and blank test solution synchronously with the series of standard solutions. The instrument automatically calculates the mass concentration of each element in the test solution based on the working curve.
[0020] 6. Experimental data processing
[0021] The mass fraction of iron w is calculated as follows, and the value is expressed in %:
[0022] Where:
[0023] ω—respectively represents the mass fraction of iron, in micrograms per gram (%);
[0024] ρ0—mass concentration of blank solution, in micrograms per liter (μg / L);
[0025] ρ1—mass concentration of the sample solution, in micrograms per liter (μg / L);
[0026] V—test volume of the sample, in milliliters (mL);
[0027] m—mass of the sample, in grams (g).
[0028] The result is rounded to two significant figures.
[0029] (3) Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. In the present invention, the lithium carbonate sample is dissolved in dilute nitric acid, boiled at low temperature to a small volume, and then 45 SC was used as an internal standard to eliminate the matrix interference of lithium. On the inductively coupled plasma mass spectrometer, a dynamic reaction cell mode was adopted, and ammonia was used as the reaction gas to produce a gas phase chemical reaction with the interfering ions to generate non-interfering substances with other mass numbers, and the iron content was quickly determined on the inductively coupled plasma mass spectrometer.
[0031] 2. The determination method of the present invention is accurate and reliable, with a detection limit of 0.00001%, a relative standard deviation of less than 20% for determining trace iron in lithium carbonate for batteries, and a spike recovery rate of 82.5% to 125.5%. Experiments have shown that the present invention is fast and accurate in determining the trace iron content in lithium carbonate for batteries, and can meet the determination of 0.00001% to 0.025% iron in lithium carbonate, and has the characteristics of low detection limit, fast analysis speed, accuracy and practicality.
[0032] 3. ICP-MS is used to determine the trace iron content in lithium carbonate for batteries. The method is fast and convenient, the results are stable and reliable, and the detection limit is as low as 0.00001%, which can meet the detection needs of lithium carbonate for batteries and even high-purity lithium carbonate with higher requirements for iron content. The method results are highly accurate and precise, solving the problem of determining trace iron in lithium carbonate for batteries.
[0033] 4. Metallic iron is relatively stable in acidic media and prevents hydrolysis. When the acid content is above 4mL (1+1) during the sample dissolution stage, the sample can be completely dissolved. As the acid content increases, the proportion of iron content in the blank in the sample measurement value increases from 13% to 32%. A large blank value will cause a great error in the sample test results. In addition, since iron is easily hydrolyzed when the acidity is low, this test finally selects 5mL (1+1) of nitric acid dissolution test solution, that is, the final acidity of the test solution is 2.5%. Accuracy can be guaranteed.
[0034] 5. The mass spectrum interference of the trace iron determination in the lithium carbonate studied by the present invention is small, and the mass number of lithium in the sample is 7, which is far different from the mass number of iron 56, and will not cause interference in the mass number. The internal standard in ICP-MS is used to correct the change of the response signal, matrix effect, atomization effect, ionization effect, instrument drift, etc. The calibration curve is drawn according to the ratio of the analytical signal to the internal standard signal, so the matrix suppression effect is eliminated.
[0035] 6. The present invention uses ICP-MS to determine the iron content in lithium carbonate samples for batteries, and the relative deviation of the determination is less than 20%. The result has good precision and meets the determination requirements.
[0036] 7. The trace iron content in lithium carbonate for battery was determined by inductively coupled plasma mass spectrometry. The recovery rate of the spiked samples was between 76% and 124%, and the results met the determination requirements. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0038] Example:
[0039] A method for determining the trace iron content in lithium carbonate for batteries, wherein the determination is carried out based on the detection principle of inductively coupled plasma mass spectrometry, and the method includes instrument conditions, sample processing, working curve drawing, sample measurement, calculation of analysis results, detection limit and determination lower limit of the method, sample dissolution experiment, sample acidity experiment, matrix interference and elimination, precision experiment, spike recovery experiment, etc.
[0040] 1. Instrument experimental conditions
[0041] Inductively coupled plasma mass spectrometer (NexION 350D, PE Company, USA), its characteristics meet the relevant requirements of GB / T 6041.
[0042] The instrument optimization test was carried out using 1μg / L Be, Mg, In, U, and Ce standard solutions. When Ce++ / Ce<3% and CeO / Ce<3%, the best working conditions of the instrument were selected based on the principle of high sensitivity and good stability. When considering the best match of sensitivity and stability, the instrument measurement conditions are shown in Table 1.
[0043] Table 1 ICP-MS operating parameters
[0044]
[0045] Selection of analytical mass number: The selection of mass number follows the principle of high abundance and less interference.
[0046] for: 56 Fe.
[0047] 2. Sample processing
[0048] 1. Sample processing: lithium carbonate sample.
[0049] Weigh 0.2000g lithium carbonate sample into a 200ml beaker, add first-grade water to completely soak the sample, slowly titrate 5mL of dilute nitric acid (1+1), cover with a watch glass, place the beaker on a hot plate and heat it to a small volume at low temperature, remove the beaker and cool it to room temperature, then transfer the solution in the beaker into a 100mL volumetric flask, dilute to the scale with first-grade water, and mix well.
[0050] 2. Reagent blank test: Add 5 mL of dilute nitric acid (1+1) to a 200 mL beaker, cover with a watch glass, place the beaker on a hot plate and heat to a small volume at low temperature, remove the beaker and cool to room temperature, rinse the beaker wall and watch glass with a wash bottle filled with first-grade water, continue to boil on the hot plate, remove the beaker and cool to room temperature, transfer the solution in the beaker to a 100 mL volumetric flask, dilute to the scale with first-grade water, and mix well.
[0051] 3. Working curve drawing
[0052] 1. Configuration of standard series solutions
[0053] Standard storage solution: Iron and scandium, use valid, certified single-element standard storage solution with a mass concentration of 1000 μg / mL.
[0054] Iron standard solution A: Pipette 1.00 mL of the iron standard stock solution into a 100 mL volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix. This solution contains 10 μg of iron per mL.
[0055] Iron standard solution B: Pipette 1.00 mL of iron standard solution into a 100 mL volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix well. This solution contains 100 μg of iron in 1 L.
[0056] Scandium internal standard solution: dilute the scandium standard stock solution (1) stepwise, and each liter of the diluted solution contains 10 μg of scandium. The medium is nitric acid (2+98).
[0057] 2. Draw the working curve: Pipette 0mL, 0.50mL, 1.00mL, 5.00mL, 10.00mL, 20.00mL, and 50.00mL of 100μg / L iron standard solution B into a set of 100mL volumetric flasks, add 2mL of concentrated nitric acid, dilute to scale with first-grade water, and mix well. This standard solution contains 0μg, 0.5μg, 1.0μg, 5.0μg, 10.0μg, 20.0μg, and 50.0μg of iron per liter.
[0058] 3. On the inductively coupled plasma mass spectrometer, after the instrument runs stably, according to the selected conditions, use the working curve method and the online addition of scandium internal standard solution, select the dynamic reaction cell (DRC) mode, use ammonia as the reaction gas, and measure the series of standard solutions. The instrument automatically draws the working curve. The correlation coefficient of the working curve of each element should be above 0.999, otherwise it is necessary to re-standardize or re-configure the series of standard solutions for standardization.
[0059] 4. Sample measurement:
[0060] On the inductively coupled plasma mass spectrometer, after the instrument runs stably, under the same conditions as in 3.3, drawing the working curve, the working curve method and the online addition of the scandium internal standard solution are used, the dynamic reaction cell (DRC) mode is selected, ammonia is used as the reaction gas, and the test solution and blank test solution are measured synchronously with the series of standard solutions. The instrument automatically calculates the mass concentration of each element in the test solution based on the working curve.
[0061] 5. Calculation of analysis results
[0062] The mass fraction of iron w is calculated as follows, and the value is expressed in %:
[0063] Where:
[0064] ω—respectively represents the mass fraction of iron, in micrograms per gram (%);
[0065] ρ0—mass concentration of blank solution, in micrograms per liter (μg / L);
[0066] ρ1—mass concentration of the sample solution, in micrograms per liter (μg / L);
[0067] V—test volume of the sample, in milliliters (mL);
[0068] m—mass of the sample, in grams (g).
[0069] The result is rounded to two significant figures.
[0070] 6. Detection limit and lower limit of determination of the method
[0071] Under the working conditions of the instrument, a blank solution without the element to be measured was used for 11 consecutive measurements, 3 times the standard deviation of the measurement result was used as the detection limit, and 10 times the standard deviation was used as the determination lower limit of the method, the detection limit: 0.066μg / L; the determination lower limit: 0.220μg / L, the detection lower limit of the method: 0.00001%. Specific data are shown in Table 2.
[0072] Table 2 Blank solution determination results
[0073]
[0074] 7. Effect of acidity on the determination results
[0075] Metallic iron is relatively stable in acidic media and prevents hydrolysis. Generally, nitric acid is the first choice, followed by hydrochloric acid. Since lithium carbonate samples are easily soluble in acid, other acids such as hydrofluoric acid, perchloric acid, sulfuric acid, and phosphoric acid are not considered in this test.
[0076] Weigh 0.2000g of sample and place it in a 200mL beaker. Add different amounts of nitric acid solution. According to the sample processing steps, the measurement is carried out under the selected instrument working conditions. The amount of acid added and the measurement results are shown in Table 3.
[0077] Table 3 Effect of acid on test results
[0078]
[0079]
[0080] The test results show that when the acid content is above 4mL (1+1) during the sample dissolution stage, the sample can be completely dissolved. As the acid content increases, the proportion of iron content in the blank in the sample measurement value increases from 13% to 32%. A large blank value will cause a great error in the sample test results. In addition, since iron is easily hydrolyzed when the acidity is low, this experiment finally selected 5mL (1+1) of nitric acid dissolution test solution, that is, the final acidity of the test solution is 2.5%.
[0081] 8. Lithium matrix interference and elimination and selection of internal standard elements
[0082] The mass spectrum interference of the trace iron determination in lithium carbonate studied by the present invention is small, and the mass number of lithium in the sample is 7, which is far different from the mass number of iron 56, and will not cause interference in the mass number. The internal standard in ICP-MS is used to correct the change of the response signal, matrix effect, atomization effect, ionization effect, instrument drift, etc. The calibration curve is drawn according to the ratio of the analytical signal to the internal standard signal, so the matrix suppression effect is eliminated.
[0083] Commonly used internal standard elements are: Sc, Ge, Y, Rh, In, Bi, etc. According to the principle of similar mass numbers, the mass number of iron in this experiment is 56, so scandium 45, which is relatively close, is selected.
[0084] IX. Precision Test
[0085] Weigh 0.2000 g of each of three different lithium carbonate samples, and perform 11 independent measurements under the selected instrument working conditions according to the sample processing steps. The experimental results are shown in Table 4.
[0086] Table 4 Sample determination results and precision
[0087]
[0088] The iron content in lithium carbonate samples for battery was determined by ICP-MS, and the relative deviation was less than 20%. The result had good precision and met the requirements for determination.
[0089] 10. Spike recovery experiment
[0090] Weigh 0.2000g of lithium carbonate sample for battery, add different amounts of iron standard solution respectively, measure under the selected instrument working conditions according to the sample processing steps, and calculate the recovery rate of iron. The measurement results are shown in Table 5.
[0091] Table 5 Iron spike recovery
[0092]
[0093] The trace iron content in lithium carbonate for battery was determined by plasma mass spectrometry. The recovery rate of the spiked samples was between 76% and 124%, and the results met the determination requirements.
[0094] The above experimental results show that the ICP-MS method for determining trace iron content in lithium carbonate for batteries is fast and convenient, the results are stable and reliable, and the detection limit is as low as 0.00001%, which can meet the detection needs of lithium carbonate for batteries and even high-purity lithium carbonate with higher requirements for iron content. The method results are highly accurate and precise, solving the problem of determining trace iron in lithium carbonate for batteries.
[0095] The above are only preferred embodiments of the present invention.
Claims
1. A method for determining trace iron content in lithium carbonate for batteries, characterized in that: The following steps are involved: (1) Sample preparation: Weigh 0.2000 g of lithium carbonate sample into a 200 ml beaker, add first-grade water to completely wet the sample, slowly titrate 5 ml of dilute nitric acid (1+1), cover with a watch glass, place the beaker on a hot plate and heat it to a small volume at low temperature, remove the beaker and cool it to room temperature, transfer the solution in the beaker into a 100 ml volumetric flask, dilute to the mark with first-grade water, mix well, and obtain a sample solution. (2) Reagent blank test: Add 5 mL of dilute nitric acid (1+1) to a 200 mL beaker, cover with a watch glass, place the beaker on a hot plate and heat to a small volume at low temperature, remove the beaker and cool to room temperature, rinse the beaker wall and watch glass with a wash bottle filled with first-grade water, continue to boil on the hot plate, remove the beaker and cool to room temperature, transfer the solution in the beaker to a 100 mL volumetric flask, dilute to the mark with first-grade water, and mix well to obtain a blank test solution. (3) Preparation of series standard solutions Standard storage solution: Iron and scandium use single element standard storage solution with a mass concentration of 1000μg / mL. Iron standard solution A: Pipette 1.00 mL of the iron standard storage solution into a 100 mL plastic volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix well. 1 mL of this solution contains 10 μg of iron. Iron standard solution B: Pipette 1.00 mL of iron standard solution A into a 100 mL plastic volumetric flask, add 2 mL of nitric acid, dilute to scale with water, and mix well. This solution contains 100 μg of iron in 1 L. Scandium internal standard solution: dilute the scandium standard storage solution step by step, and each liter of the diluted solution contains 10 μg of scandium. The medium is nitric acid (2+98). (4) Draw a working curve: Pipette 0 mL, 0.50 mL, 1.00 mL, 5.00 mL, 10.00 mL, 20.00 mL, and 50.00 mL of 100 μg / L iron standard solution B into a set of 100 mL plastic volumetric flasks, add 2 mL of nitric acid, dilute to scale with first-grade water, and mix well. This standard solution contains 0 μg, 0.5 μg, 1.0 μg, 5.0 μg, 10.0 μg, 20.0 μg, and 50.0 μg of iron per liter. An inductively coupled plasma mass spectrometer was selected, and the measurement parameters were as follows: high frequency generator power 1300w, cooling gas 18.0L / min, auxiliary gas 1.2L / min, nebulizer gas 0.82L / min, measurement mode pulse, and analysis mass number 56 Fe, on an inductively coupled plasma mass spectrometer, after the instrument runs stably, use the working curve method and the online addition of scandium internal standard solution, select the dynamic reaction cell mode, use ammonia as the reaction gas, measure the series of standard solutions, and the instrument automatically draws the working curve. The correlation coefficient of the working curve should be above 0.999, otherwise it is necessary to re-standardize or re-configure the series of standard solutions for standardization. (5) On an inductively coupled plasma mass spectrometer, under the same conditions as step (4), the sample solution and the blank test solution are measured synchronously with the series of standard solutions by using the working curve method and online addition of the scandium internal standard solution. The instrument automatically calculates the mass concentration of each element in the test solution based on the working curve. (6) Experimental data processing The mass fraction of iron w is calculated as follows, with the numerical unit expressed in μg / g: Where: w—respectively the mass fraction of iron, in micrograms per gram μg / g; ρ0—mass concentration of blank solution, in micrograms per liter μg / L; ρ1—mass concentration of sample solution, in micrograms per liter μg / L; V—measured volume of sample, in milliliters mL; m—mass of the sample, in grams.