Additive method for preparing large-size metal grid transparent electrode

The additive method uses a combination of single-sided tape and double-sided film to directly print and solidify copper enameled wires, which solves the problems of waste of metal materials and complex processes in the traditional etching process, and achieves efficient and environmentally friendly preparation of large-size metal grid transparent electrodes. , suitable for mass production.

CN118866433APending Publication Date: 2024-10-29MICRON OPTOELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411265534.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Traditional etching methods waste a lot of metal materials when preparing metal mesh transparent electrodes, and the production process is complex, which limits production efficiency and product consistency.

Method used

Using the additive method, a single-sided adhesive base film and a double-sided film are used to directly print the copper enameled wire through the printing equipment and fix it through the UV curing process, simplifying the process and reducing material waste and process steps.

Benefits of technology

It reduces material costs, improves production efficiency and the mechanical and environmental stability of the product, is suitable for mass production, and can customize the performance of large-size transparent electrodes according to different application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118866433A_ABST
    Figure CN118866433A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a large-size metal grid transparent electrode through an additive method.The method comprises the following steps that S1, a base film with glue on a single face is selected, the high transmittance of the base film is larger than 89%, the high viscosity of the base film is larger than 1800 gf / 25 mm, and the base film can be used for bonding a copper enameled wire with the width ranging from 5 micrometers to 30 micrometers; s2, directly printing the copper enameled wire on the adhesive surface of the base film by using printing equipment according to a preset direction and a preset wiring rule; s3, after printing is completed, a layer of double-sided film is attached to the surface of the copper wire; through a mode of directly printing the copper enameled wire, waste of a large amount of copper in a traditional etching process is avoided, the material cost is reduced, the combination of the single-sided adhesive base film and the double-sided film is used, the use amount of the optical transparent adhesive is reduced, the cost is further reduced, the production process is simplified, and due to the fact that the arrangement of the copper wires can be flexibly designed, the production efficiency is improved. Therefore, the performance of the large-size transparent electrode can be customized according to different application requirements, the method is environment-friendly, efficient and suitable for large-scale production, and the product has good environmental stability and mechanical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic materials and optoelectronic devices, and in particular to the preparation of large-size metal grid transparent electrodes by an additive method. Background Art

[0002] Transparent electrodes are components that have both high conductivity and high visible light transmittance. They play a vital role in optoelectronic devices such as solar cells, touch screens, and light-emitting diodes. Traditional ITO electrodes are being replaced by new materials, including metal grid transparent electrodes, due to their poor mechanical strength and flexibility, as well as concerns about cost and sustainability.

[0003] Existing etching methods waste a large amount of metal materials, especially copper, when preparing metal grids, and cause environmental pollution; current production processes such as electroplating and chemical plating often require multiple steps, involve delicate and complex operations, and have strict requirements on manufacturing conditions, which limits production efficiency and product consistency. Summary of the Invention

[0004] The purpose of the present invention is to provide a method for preparing a large-size metal grid transparent electrode by an additive method to solve the problems raised in the above background technology.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a large-size metal grid transparent electrode is prepared by an additive method, the method comprising the following steps:

[0006] S1: Select a single-sided adhesive base film with a high transmittance greater than 89% and a high viscosity greater than 1800gf / 25mm, capable of bonding copper enameled wire with a width of 5-30μm;

[0007] S2: Use a printing device to print the copper enameled wire directly on the adhesive surface of the base film according to the preset direction and wiring rules;

[0008] S3: After printing is completed, a double-sided film is applied to the surface of the copper wire. This double-sided film can not only fix the copper wire, but also serve as a medium for bonding the cover plate in subsequent processing;

[0009] S4: Ensure the strong bond between the copper wire, base film and double-sided film through the UV curing process;

[0010] S5: Post-process the prepared metal grid transparent electrode to ensure product quality.

[0011] Preferably, the method for preparing the base film with adhesive on one side comprises the following steps:

[0012] S11: Selecting nano-scale materials with high light transmittance as the main component of the base film to improve the transmittance of the base film.

[0013] S12: Through surface modification technology, the dispersibility of nanomaterials is optimized to ensure uniform distribution in the base film, thereby avoiding light scattering and reduced transmittance due to agglomeration.

[0014] S13: Using a specific resin and additive formula, the viscosity of the base film is adjusted to achieve a viscosity requirement greater than 1800gf / 25mm while maintaining high transparency, to facilitate accurate printing and bonding of copper wire.

[0015] S14: Using high-speed mixing and coating equipment, the above formula is mixed and coated into a film to ensure the thickness and quality of the base film.

[0016] S15: Through the UV curing process, the base film achieves the required physical and chemical stability while maintaining the high transmittance and high viscosity characteristics of the base film.

[0017] Preferably, the nano-scale material with high light transmittance includes nano-aluminum oxide and nano-silicon dioxide.

[0018] Preferably, the specific resin formula includes polymethyl methacrylate, polycarbonate, and polystyrene high transparency resin.

[0019] Preferably, the specific resin formula further includes modified epoxy resin, polyurethane resin and high-viscosity resin.

[0020] Preferably, the specific additive formulation includes hydroxymethyl cellulose and hydroxyethyl cellulose thickeners.

[0021] Preferably, the specific additive formula further includes sodium lauryl sulfate and polyethylene glycol dispersant.

[0022] Preferably, the post-processing includes cutting, cleaning and inspection.

[0023] Preferably, the double-sided film is added with nano-silicone nanoparticles and conductive polymer functional materials, which can improve the mechanical properties of the double-sided film and enhance the adhesion between the double-sided film and the copper wire.

[0024] Preferably, the structure of the copper enameled wire adopts a multi-strand copper wire braided structure to improve the adhesion of the copper enameled wire on the base film.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention avoids the large amount of copper waste in traditional etching processes by directly printing copper enameled wires, reducing material costs. The combination of a single-sided adhesive base film and a double-sided film reduces the amount of optically transparent adhesive used, further reducing costs and simplifying the production process. Since the layout of the copper wires can be flexibly designed, the performance of large-size transparent electrodes can be customized according to different application requirements. This method is environmentally friendly, efficient, suitable for large-scale production, and the product has good environmental stability and mechanical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a process diagram for the additive manufacturing of large-size metal grid transparent electrodes according to the present invention. DETAILED DESCRIPTION

[0028] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0029] See also Figure 1 The present invention provides a technical solution: preparing a large-size metal grid transparent electrode by an additive method, the method comprising the following steps:

[0030] S1: Select a single-sided adhesive base film with a high transmittance greater than 89% and a high viscosity greater than 1800gf / 25mm, capable of bonding copper enameled wire with a width of 5-30μm;

[0031] S2: Use a printing device to print the copper enameled wire directly on the adhesive surface of the base film according to the preset direction and wiring rules;

[0032] S3: After printing is completed, a double-sided film is applied to the surface of the copper wire. This double-sided film can not only fix the copper wire, but also serve as a medium for bonding the cover plate in subsequent processing;

[0033] S4: Ensure the strong bond between the copper wire, base film and double-sided film through the UV curing process;

[0034] S5: Post-process the prepared metal grid transparent electrode to ensure product quality.

[0035] Post-processing includes cutting, cleaning and inspection; the cutting process cuts the metal mesh transparent electrode into the required large size as needed. During the cutting process, the edges must be neat and the copper wire must not be damaged; the cleaning process uses solvents to clean the electrode surface to remove residual adhesives and impurities to ensure the cleanliness and surface quality of the electrode; the inspection process performs various performance tests on the metal mesh transparent electrode, including transmittance, conductivity, and mechanical strength, to ensure that the product quality meets the requirements.

[0036] The addition of nanosilicone nanoparticles and conductive polymer functional materials to the double-sided film can improve the mechanical properties of the double-sided film and enhance the adhesion between the double-sided film and the copper wire.

[0037] The structure of the copper enameled wire adopts a multi-strand copper wire braiding structure to improve the adhesion of the copper enameled wire to the base film.

[0038] The method for preparing a base film with adhesive on one side comprises the following steps:

[0039] S11: Selecting nano-scale materials with high light transmittance as the main component of the base film to improve the transmittance of the base film.

[0040] S12: Through surface modification technology, the dispersibility of nanomaterials is optimized to ensure uniform distribution in the base film, thereby avoiding light scattering and reduced transmittance due to agglomeration.

[0041] S13: Using a specific resin and additive formula, the viscosity of the base film is adjusted to achieve a viscosity requirement greater than 1800gf / 25mm while maintaining high transparency, to facilitate accurate printing and bonding of copper wire.

[0042] S14: Using high-speed mixing and coating equipment, the above formula is mixed and coated into a film to ensure the thickness and quality of the base film.

[0043] S15: Through the UV curing process, the base film achieves the required physical and chemical stability while maintaining the high transmittance and high viscosity characteristics of the base film.

[0044] Nano-scale materials with high light transmittance include nano-alumina and nano-silica; specific resin formulas include polymethyl methacrylate, polycarbonate, and polystyrene high-transparency resins, as well as modified epoxy resins and polyurethane resins with high viscosity; specific additive formulas include hydroxymethyl cellulose and hydroxyethyl cellulose thickeners, as well as sodium lauryl sulfate and polyethylene glycol dispersants.

[0045] By disclosing a method for preparing a high-transmittance and high-viscosity base film based on a new nano-composite material, a base film that can maintain both high transmittance and high viscosity is prepared by using nano-scale transparent materials and an optimized resin formula, which is used for additive manufacturing of large-size metal grid transparent electrodes.

[0046] In summary, the present invention avoids the large amount of copper waste in the traditional etching process by directly printing the copper enameled wire, reduces material costs, uses a combination of a single-sided adhesive base film and a double-sided film, reduces the amount of optically transparent adhesive used, further reduces costs and simplifies the production process. Since the layout of the copper wire can be flexibly designed, the performance of large-size transparent electrodes can be customized according to different application requirements. This method is environmentally friendly, efficient, suitable for large-scale production, and the product has good environmental stability and mechanical stability.

[0047] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. Additive method for preparing large-size metal grid transparent electrodes, characterized in that: The method comprises the following steps: S1: Select a single-sided adhesive base film, which has a high transmittance greater than 89% and a high viscosity greater than 1800gf / 25mm, and can bond copper enameled wires with a width of 5-30μm; S2: Use a printing device to directly print the copper enameled wire on the adhesive surface of the base film according to the preset direction and wiring rules; S3: After printing, a double-sided film is attached to the surface of the copper wire. The double-sided film can not only fix the copper wire, but also serve as a medium for bonding the cover plate in subsequent processing; S4: Ensure the strong bonding between the copper wire, the base film and the double-sided film through the UV curing process; S5: Post-process the prepared metal grid transparent electrode to ensure product quality.

2. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 1, characterized in that: The method for preparing the single-sided adhesive base film comprises the following steps: S11: Selecting nano-scale materials with high light transmittance as the main component of the base film to improve the transmittance of the base film. S12: Through surface modification technology, the dispersibility of nanomaterials is optimized to ensure uniform distribution in the base film, thereby avoiding light scattering and reduced transmittance due to agglomeration. S13: A specific resin and additive formula is used to adjust the viscosity of the base film so that it can reach a viscosity requirement of more than 1800gf / 25mm while maintaining high transparency, so as to facilitate the precise printing and bonding of copper wires. S14: Using high-speed mixing and coating equipment, the above formula is mixed and coated into a film to ensure the thickness and quality of the base film. S15: Through the UV curing process, the base film achieves the required physical and chemical stability while maintaining the high transmittance and high viscosity characteristics of the base film.

3. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 2, characterized in that: The nano-scale materials with high light transmittance include nano-aluminum oxide and nano-silicon dioxide.

4. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 2, characterized in that: The specific resin formulation includes polymethyl methacrylate, polycarbonate, and polystyrene high transparency resin.

5. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 2, characterized in that: The specific resin formulation also includes modified epoxy resin, polyurethane resin and high viscosity resin.

6. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 2, characterized in that: The specific additive formulation includes hydroxymethyl cellulose and hydroxyethyl cellulose thickeners.

7. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 2, characterized in that: The specific additive formula also includes sodium lauryl sulfate and polyethylene glycol dispersant.

8. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 1, characterized in that: The post-processing includes cutting, cleaning and inspection.

9. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 1, characterized in that: The double-sided film is added with nano-silicone nanoparticles and conductive polymer functional materials, which can improve the mechanical properties of the double-sided film and enhance the adhesion between the double-sided film and the copper wire.

10. The method for preparing a large-size metal grid transparent electrode by additive manufacturing according to claim 1, characterized in that: The structure of the copper enameled wire adopts a multi-strand copper wire braiding structure to improve the adhesion of the copper enameled wire on the base film.