Electrolyte, lithium ion battery and electric equipment

By adding dissolved oxygen and ozone to the electrolyte and optimizing the SEI structure, the problem of poor low-temperature performance of lithium iron phosphate batteries is solved, and better low-temperature discharge capabilities and cruising range are achieved.

CN118867375AActive Publication Date: 2024-10-29BYD CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310489027.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-29
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Lithium iron phosphate batteries have poor discharge capacity at low temperatures, which affects the cruising range of electric vehicles. It is difficult for existing additives to effectively solve low-temperature performance issues.

Method used

Provide an electrolyte containing dissolved oxygen, lithium salt and organic solvent, the dissolved oxygen includes oxygen and ozone, adjust the molar ratio of oxygen and ozone through ultraviolet radiation, optimize the SEI structure of the negative electrode side, and reduce the battery impedance.

Benefits of technology

It significantly improves the low-temperature discharge capability of lithium-ion batteries, reduces the battery's impedance at low temperatures, and improves low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867375A_ABST
    Figure CN118867375A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion battery, in particular to an electrolyte, a lithium ion battery and electric equipment. The electrolyte provided by the invention contains dissolved oxygen, lithium salt and an organic solvent, wherein the dissolved oxygen comprises oxygen. The electrolyte is injected into the lithium ion battery, and in the formation process of the lithium ion battery, the lithium ion battery has relatively high low-temperature capacity retention rate and cycle capacity retention rate by optimizing an SEI structure on the surface of a negative electrode and reducing the impedance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium ion battery, in particular to an electrolyte, a lithium ion battery containing the electrolyte, and an electrical device containing the lithium ion battery. Background Art

[0002] Batteries with lithium iron phosphate (LiFePO4) as the positive electrode active material are widely used in electric vehicles and energy storage systems. However, the discharge capacity of lithium iron phosphate batteries is significantly reduced at low temperatures, that is, the low-temperature discharge capacity is poor, which reduces the cruising range of electric vehicles under low temperature conditions and affects the user experience. There are many factors that affect the low-temperature performance of lithium iron phosphate batteries, such as the structure of the positive electrode material, the migration rate of lithium ions inside the battery, the chemical composition of the SEI film, and the selection of lithium salts and solvents in the electrolyte. Among them, introducing functional additives into the electrolyte of the battery is considered to be one of the effective ways to improve the low-temperature performance of lithium iron phosphate batteries. However, there are many types of additives, and additives with a single function are difficult to solve the problem; additives with complex formula combinations will have system compatibility problems, resulting in insufficient other battery performance and failure to achieve the purpose of use.

[0003] Therefore, there is an urgent need to develop a new electrolyte that can effectively improve the low-temperature performance of lithium iron phosphate lithium-ion batteries. Summary of the invention

[0004] The purpose of the present invention is to overcome the low-temperature discharge performance of existing lithium iron phosphate batteries and to provide an electrolyte, a lithium ion battery containing the electrolyte, and an electrical device containing the lithium ion battery.

[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides an electrolyte, which contains dissolved oxygen, a lithium salt and an organic solvent; wherein the dissolved oxygen includes oxygen gas.

[0006] Preferably, the concentration of dissolved oxygen in the electrolyte is 0.001-0.1 mol / L, preferably 0.005-0.05 mol / L.

[0007] Preferably, the dissolved oxygen also includes ozone.

[0008] Preferably, the ozone in the dissolved oxygen is obtained by subjecting the dissolved oxygen to ultraviolet radiation.

[0009] Preferably, in the dissolved oxygen, the molar ratio of oxygen to ozone is 1:0.001-1, preferably 1:0.005-0.1, and more preferably 1:0.01-0.1.

[0010] Preferably, the conditions of ultraviolet radiation include: ultraviolet wavelength is 10-400nm, preferably 100-400nm; the power of the ultraviolet generator is 10-3000W, preferably 60-600W; ultraviolet radiation time is 0.1-1000min, preferably 1-100min.

[0011] A second aspect of the present invention provides a lithium-ion battery, which comprises a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte provided in the first aspect.

[0012] Preferably, the lithium-ion battery is subjected to formation to form a SEI film on the surface of the negative electrode plate.

[0013] Preferably, the formation temperature is 20-40°C, preferably 20-30°C.

[0014] Preferably, the SEI film contains Li2O; based on the total weight of the SEI film, the content of Li2O is 10-40wt%, preferably 15-35wt%.

[0015] Preferably, the SEI film further contains Li2CO3; based on the total weight of the SEI film, the content of Li2CO3 is 40-80wt%, preferably 50-70wt%.

[0016] Preferably, the thickness of the SEI film is 2-200 nm, preferably 10-100 nm.

[0017] A fourth aspect of the present invention provides an electrical device, wherein the electrical device comprises the lithium-ion battery provided in the third aspect.

[0018] Through the above technical scheme, the electrolyte provided by the present invention contains dissolved oxygen, and the dissolved oxygen in the electrolyte can optimize the SEI structure and composition on the negative electrode side, thereby reducing the battery impedance, especially reducing the impedance of the battery at low temperatures; thereby improving the low-temperature discharge capacity of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a photoelectron spectroscopy (XPS) spectrum of the SEI film of the finished lithium-ion battery Q1 containing the electrolyte S1 of Example 1;

[0020] Figure 2 It is a photoelectron spectroscopy (XPS) spectrum of the SEI film of the finished lithium-ion battery DQ1 containing the electrolyte DS1 of Comparative Example 1. DETAILED DESCRIPTION

[0021] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0022] A first aspect of the present invention provides an electrolyte, the electrolyte containing dissolved oxygen, a lithium salt and an organic solvent; wherein the dissolved oxygen includes oxygen.

[0023] The inventors of the present invention have found through research that by dissolving a certain proportion of oxygen in the electrolyte in advance, the proportion of oxygen in the electrolyte is much higher than that of the normal electrolyte without pre-dissolving oxygen. The resulting lithium-ion battery has lower impedance, especially under low temperature conditions, the impedance increase ratio is reduced, and has better low-temperature discharge capability.

[0024] In some embodiments of the present invention, preferably, the dissolved oxygen also includes ozone.

[0025] In the present invention, unless otherwise specified, the ozone in the dissolved oxygen may be introduced separately or converted from the oxygen in the electrolyte. That is, the electrolyte provided by the present invention is in an oxygen-rich environment, the oxygen in the electrolyte is in a saturated state, and when part of the oxygen is converted into ozone, a corresponding part of the oxygen will dissolve, so that the oxygen and ozone in the dissolved oxygen are in a dynamic equilibrium state.

[0026] In the present invention, unless otherwise specified, the dissolved oxygen includes oxygen and ozone, which means that the dissolved oxygen is a mixed gas of oxygen and ozone, and oxygen and ozone are in a dynamic equilibrium state. Preferably, the dissolved oxygen consists of oxygen and ozone.

[0027] In some embodiments of the present invention, preferably, the concentration of dissolved oxygen in the electrolyte is 0.001-0.1 mol / L, for example, 0.001 mol / L, 0.005 mol / L, 0.01 mol / L, 0.015 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, and any value in the range of any two values, preferably 0.005-0.05 mol / L. When the dissolved oxygen is within the above range, the dissolved oxygen can be completely consumed during battery formation and will not affect the subsequent use of the battery.

[0028] In some embodiments of the present invention, preferably, the ozone in the dissolved oxygen is obtained by ultraviolet radiation of the dissolved oxygen. In the present invention, part of the dissolved oxygen is converted into ozone by ultraviolet irradiation, and the molar ratio of ozone to oxygen in the dissolved oxygen is adjusted so that the proportion of oxygen or ozone in the electrolyte is much higher than that of a normal electrolyte that is not pre-dissolved.

[0029] In some embodiments of the present invention, preferably, in the dissolved oxygen, the molar ratio of oxygen to ozone is 1:0.001-1, for example, 1:0.001, 1:0.005, 1:0.01, 1:0.012, 1:0.015, 1:0.03, 1:0.05, 1:0.08, 1:0.1, 1:0.5, 1:1, and any value in the range of any two values, preferably 1:0.005-0.1, more preferably 1:0.01-0.1. When the molar ratio of oxygen to ozone in the dissolved oxygen is less than 1:0.001, the ozone concentration is too low, and the effect of reducing the low-temperature impedance of the battery is not obvious; when the molar ratio of oxygen to ozone in the dissolved oxygen is greater than 1:1, the ozone concentration is too high, the electrolyte side reaction increases, and the battery performance deteriorates.

[0030] In the present invention, unless otherwise specified, the oxygen concentration in the electrolyte is measured using a static phase equilibrium method, and the ozone concentration is measured using CJ / T 3028.2-94; the test temperature is room temperature (ie, 25-30° C.).

[0031] In some embodiments of the present invention, preferably, the conditions of ultraviolet radiation include: ultraviolet wavelength is 10-400nm; the power of ultraviolet generator is 10-3000W; ultraviolet radiation time is 0.1-1000min.

[0032] In some embodiments of the present invention, further preferably, the conditions of the ultraviolet radiation include: the ultraviolet wavelength is 100-400nm; the power of the ultraviolet generator is 60-600W; and the ultraviolet radiation time is 1-100min.

[0033] In some embodiments of the present invention, preferably, the concentration of the lithium salt in the electrolyte is 5-30wt%, for example, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, and any value in the range composed of any two values, preferably 7-20wt%.

[0034] In the present invention, the type of the lithium salt has a wide range of selection. Preferably, the lithium salt is selected from at least one of LiPF6, LiAsF6, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide and their derivatives; further preferably, the lithium bis(trifluoromethylsulfonyl)imide derivative is selected from at least one of lithium bis(pentafluoroethylsulfonyl)imide, lithium trifluoromethylsulfonyl-pentafluoroethylsulfonylimide and lithium fluorosulfonyl trifluoromethylsulfonylimide.

[0035] In some embodiments of the present invention, preferably, the organic solvent is selected from at least one of ether compounds, ester compounds, amide compounds, nitrile compounds and aromatic compounds, preferably selected from ether compounds and / or ester compounds.

[0036] In some embodiments of the present invention, preferably, the ether compound is selected from at least one of cyclic ethers, linear ethers and fluorinated ethers; further preferably, the cyclic ether is selected from at least one of 1,3-dioxolane, 1,4-dioxane, tetrahydrofuran, tetrahydropyran and propylene oxide; the linear ether is selected from at least one of methyl glycol dimethyl ether, methyl glycol diethyl ether, ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether, ethylene glycol methyl ethyl ether, tert-butyl methyl ether, tert-butyl ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and dipropylene glycol dimethyl ether; the fluorinated ether is selected from at least one of bis-2,2 - At least one of trifluoroethyl ether (BTFE), 1,1,1,2,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, nonafluorobutyl methyl ether, nonafluorobutyl ethyl ether, nonafluorobutyl propyl ether, n-butyl-1,1,2,2-tetrafluoroethyl ether, 2,2,3,3,3-pentafluoropropyl methyl ether, 2,1,2,2-tetrafluoroethyl ether, 1,1,2,2-tetrafluoroethyl methyl ether, 1,1,2,2-tetrafluoroethyl ethyl ether and trifluoroethyl dodecafluorohexyl ether.

[0037] According to a preferred embodiment of the present invention, the organic solvent is a linear ether and a cyclic ether, wherein the weight ratio of the linear ether to the cyclic ether is 10-50:50-90, preferably 25-50:50-75. The use of a mixture of a cyclic ether compound and a linear ether with a lower reduction potential in a preferred ratio can prepare an electrolyte with higher stability to lithium and prevent the reduction reaction of the electrolyte at the negative electrode.

[0038] In some embodiments of the present invention, preferably, the ester compound is selected from inorganic acid esters and / or organic acid esters, the inorganic acid esters are preferably selected from carbonates and / or phosphates, and the carbonates are selected from cyclic carbonates and / or linear carbonates.

[0039] In some embodiments of the present invention, further preferably, the organic acid ester is selected from at least one of methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, methyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone and ε-caprolactone; more preferably, the organic acid ester is selected from at least one of ethyl propionate, propyl propionate and methyl propionate. The preferred conditions are more conducive to reducing the viscosity of the electrolyte.

[0040] In some embodiments of the present invention, further preferably, the cyclic carbonate is selected from at least one of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate, and their halides; the linear carbonate is selected from at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate and methyl propyl carbonate.

[0041] According to a preferred embodiment of the present invention, the organic solvent is a cyclic carbonate and a linear carbonate, wherein the weight ratio of the cyclic carbonate to the linear carbonate is 10-50:50-90, preferably 25-50:50-75. Under the preferred conditions, the combination of a high dielectric constant cyclic carbonate and a low viscosity linear carbonate is more conducive to improving the ionic conductivity of the electrolyte and preventing the reduction reaction of the electrolyte at the negative electrode.

[0042] In some embodiments of the present invention, further preferably, the phosphate is selected from at least one of trimethylphosphine oxide, triethylphosphine oxide, tripropylphosphine oxide, triphenylphosphine oxide, diethyl methylphosphonate, dimethyl methylphosphonate, diphenyl methylphosphonate, bis(2,2,2-trifluoroethyl)methylphosphonate, trimethyl phosphate, triethyl phosphate, tripropyl phosphate and ethylmethylphenyl phosphate.

[0043] In some embodiments of the present invention, preferably, the nitrile compound is selected from at least one of acetonitrile, propionitrile, butyronitrile, valeronitrile, hexanenitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorobenzoyl cyanide and 4-fluorobenzoyl cyanide.

[0044] In the present invention, the amide compounds and aromatic compounds have a wide selection range, and they are all conventional specific compounds in the art, and the present invention is not limited thereto.

[0045] In some embodiments of the present invention, preferably, the electrolyte also includes an additive; further preferably, the content of the additive in the electrolyte is 0.05-10wt%, for example, 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 3wt%, 5wt%, 8wt%, 10wt%, and any value in the range composed of any two values, preferably 0.1-5wt%.

[0046] In the present invention, the type of the additive has a wide range of selection. Preferably, the additive is selected from at least one of vinylene carbonate, ethylene carbonate, fluoroethylene carbonate, lithium difluorophosphate, lithium dioxalate borate, lithium difluorooxalate borate, 1,3-propane sultone, triallyl isocyanurate, methylene methane disulfonate, vinyl sulfate, triallyl phosphate and tripropynyl phosphate.

[0047] In the present invention, the preparation method of the electrolyte has a wide range of selection, as long as the electrolyte contains dissolved oxygen, lithium salt and organic solvent. Preferably, the preparation method of the electrolyte comprises the following steps: (1) mixing lithium salt, additive and organic solvent to obtain a mixed solution; (2) contacting and dissolving the mixed solution and oxygen in a volume ratio of 1-100:1 in a non-oxidizing atmosphere to obtain an electrolyte precursor with an oxygen solubility of 0.001-0.09 mol / L; (3) subjecting the electrolyte precursor to ultraviolet radiation in a non-oxidizing atmosphere to convert the dissolved oxygen into ozone to obtain an electrolyte with a dissolved oxygen content of 0.001-0.1 mol / L, wherein the dissolved oxygen includes oxygen and ozone, and the molar ratio of oxygen to ozone is 1:0.001-1, preferably 1:0.005-0.1, and more preferably 1:0.01-0.1.

[0048] In the present invention, unless otherwise specified, the types of lithium salts, additives and organic solvents, as well as the conditions of ultraviolet radiation are in accordance with the above-mentioned definitions, and the present invention will not be elaborated herein.

[0049] In some embodiments of the present invention, preferably, in step (1), the weight ratio of the lithium salt, the additive and the organic solvent is 1-20:0.1-10:20-100.

[0050] In some embodiments of the present invention, preferably, in step (2), the dissolution conditions include: temperature of 15-40°C, preferably 20-30°C; time of 10-40h, preferably 20-30h.

[0051] In the present invention, in step (2), the oxygen solubility refers to the solubility of oxygen when the amount of oxygen dissolved in the electrolyte precursor reaches a saturated state.

[0052] A second aspect of the present invention provides a lithium-ion battery, which comprises a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte provided in the first aspect.

[0053] In some embodiments of the present invention, preferably, the lithium-ion battery is subjected to formation to form a SEI film on the surface of the negative electrode plate. Meanwhile, during the formation of the electrolyte, the dissolved oxygen is completely consumed and will not affect the subsequent use of the battery.

[0054] In some embodiments of the present invention, preferably, the formation temperature is 20-40°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, and any value in the range consisting of any two values, preferably 20-30°C.

[0055] In some embodiments of the present invention, preferably, the SEI film contains Li2O; based on the total weight of the SEI film, the content of Li2O is 10-40wt%, for example, 10wt%, 15wt%, 25wt%, 35wt%, 40wt%, and any value in the range consisting of any two values, preferably 15-35wt%.

[0056] In some embodiments of the present invention, preferably, the SEI film also contains Li2CO3; based on the total weight of the SEI film, the content of Li2CO3 is 40-80wt%, for example, 40wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 80wt%, and any value in the range composed of any two values, preferably 50-70wt%.

[0057] In the SEI film, the content of Li2CO3 is 40-80wt%, preferably 50-70wt%; the content of Li2O is 10-40wt%, preferably 15-35wt%.

[0058] In the present invention, unless otherwise specified, the Li2CO3 content parameter and the Li2O content parameter in the SEI film are measured by XPS (X-ray photoelectron spectroscopy) peak fitting.

[0059] In the present invention, unless otherwise specified, the SEI film includes organic lithium salts in addition to Li2CO3 and Li2O.

[0060] In some embodiments of the present invention, preferably, the thickness of the SEI film is 2-200 nm, for example, 2 nm, 10 nm, 30 nm, 50 nm, 80 nm, 100 nm, 150 nm, 200 nm, and any value in the range consisting of any two values, preferably 10-100 nm.

[0061] In the present invention, unless otherwise specified, the SEI film thickness parameter is obtained by TEM (transmission electron microscope) testing.

[0062] In some embodiments of the present invention, preferably, the operating temperature of the lithium ion battery is -20°C to 65°C, for example, -20°C, -10°C, 0°C, 10°C, 20°C, 25°C, 30°C, 50°C, 65°C, and any value in the range of any two values, preferably 20-30°C.

[0063] In some embodiments of the present invention, preferably, the charge transfer impedance of the lithium ion battery at -20°C is ≤1.2Ω·Ah, for example, 0.1Ω·Ah, 0.2Ω·Ah, 0.3Ω·Ah, 0.4Ω·Ah, 0.5Ω·Ah, 0.8Ω·Ah, 1Ω·Ah and 1.2Ω·Ah, and any value in the range of any two values, preferably 0.1-0.5Ω·Ah. In the present invention, the charge transfer impedance of the lithium ion battery at -20°C is tested using an electrochemical workstation.

[0064] In some embodiments of the present invention, preferably, the capacity retention rate of the lithium ion battery at -20°C is ≥65%, preferably 65-80%; the capacity retention rate after 500 cycles at 25°C is ≥91%, preferably 93.5-97.5%.

[0065] In the present invention, unless otherwise specified, the capacity retention rate is measured using a lithium-ion battery charge and discharge test cabinet.

[0066] In the present invention, the capacity retention rate test method at different temperatures is as follows: (1) at 25±5°C, charge the battery to the upper limit voltage (0.05C current cutoff) at a constant current and constant voltage of 1 / 3C (C is the rated capacity of the battery), let it stand for 10 minutes, and then discharge it to the lower limit voltage of the battery at a constant current of 1 / 3C, and the obtained capacity is C0; (2) charge the battery to the upper limit voltage (0.05C current cutoff) at a constant current and constant voltage of 1 / 3C, transfer the battery to a constant temperature box, set the temperature of the constant temperature box to the test temperature, and let it stand for 12 hours to allow the battery temperature to reach the test temperature; (3) discharge the battery to the lower limit voltage at a constant current of 1 / 3C, and the obtained capacity is C1, and C1 / C0 is the capacity retention rate at this temperature. Repeat the above steps (1)-(3) to obtain the battery capacity retention rate at different temperatures.

[0067] In the present invention, the capacity retention rate test method for 500 cycles at 25°C is as follows: (1) at 25±5°C, charge the battery at a constant current and constant voltage of 0.5C (C is the rated capacity of the battery) to the upper limit voltage of the battery (0.05C current cutoff), and let it stand for 10 minutes; (2) discharge the battery at a constant current of 0.5C to the lower limit voltage of the battery, the capacity is C0, and let it stand for 10 minutes; repeat the above steps (1)-(2) 500 times, the discharge capacity of the 500th cycle is C500, and C500 / C0 is the capacity retention rate after 500 cycles at 25°C.

[0068] A fourth aspect of the present invention provides an electrical device, wherein the electrical device comprises the lithium-ion battery provided in the third aspect.

[0069] In the present invention, unless otherwise specified, the electrical equipment includes but is not limited to mobile phones, cars, etc.

[0070] According to a particularly preferred embodiment of the present invention, an electrolyte comprises dissolved oxygen, a lithium salt, an additive and an organic solvent; wherein the dissolved oxygen comprises oxygen and ozone, and the ozone in the dissolved oxygen is obtained by ultraviolet radiation of dissolved oxygen;

[0071] Wherein, the molar ratio of oxygen to ozone in the dissolved oxygen is 1:0.01-0.1;

[0072] Wherein, the concentration of dissolved oxygen in the electrolyte is 0.005-0.05 mol / L;

[0073] The conditions of ultraviolet radiation include: ultraviolet wavelength of 100-400nm; power of ultraviolet generator of 60-600W; ultraviolet radiation time of 1-100min.

[0074] The present invention will be described in detail below through examples.

[0075] Preparation of lithium-ion battery P1: lithium iron phosphate: PVDF: carbon nanotube: graphene: NMP = 100: 2.5: 1: 0.5: 60 weight ratio, uniformly mixed to prepare positive electrode slurry, coated on aluminum foil current collector, control the single surface density of positive electrode coating to 200g / m 2 After baking, the positive electrode sheet was obtained; at the same time, the weight ratio of graphite: CMC: SBR: carbon black: H2O = 100:3:2:1:100 was used to prepare the negative electrode slurry, which was coated on the copper foil current collector to control the single-sided surface density of the negative electrode to 100g / m 2 , and after baking, a negative electrode sheet is obtained; the positive electrode sheet and the negative electrode sheet are respectively rolled, slit, die-cut, stacked, and assembled to form a lithium-ion battery.

[0076] Example 1

[0077] (1) mixing LiPF6, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and vinylene carbonate in a weight ratio of 13:30:11:12:34:5 to obtain a mixed solution;

[0078] (2) the mixed solution was placed in a 100 L stainless steel sealed container with a filling ratio of 90%, and then 10 L of oxygen was introduced into the stainless steel sealed container and allowed to stand at 25° C. for 24 h to allow the oxygen concentration in the mixed solution to become saturated;

[0079] (3) A stainless steel sealed container is equipped with an ultraviolet lamp, the ultraviolet wavelength is controlled to be 150nm, and the ultraviolet light is radiated at a power of 200W for 1 hour, so that the remaining dissolved oxygen is radiated by external ultraviolet light to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is adjusted to be 1:0.012, thereby obtaining electrolyte S1;

[0080] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S1 is 0.012 mol / L;

[0081] (4) The electrolyte S1 was injected into the lithium-ion battery P1, and after being fully infiltrated, it was formed at 25±5°C, and then sealed after exhaust, liquid replenishment, charging, aging, capacity separation, and self-discharge testing. The finished lithium-ion battery Q1 was tested for discharge capacity at different temperatures. The test results are listed in Table 1.

[0082] Example 2

[0083] According to the method of Example 1, the difference is that

[0084] In step (3), the ultraviolet wavelength is controlled to be 200 nm, and the radiation is carried out at a power of 400 W for 1 hour, so that the remaining dissolved oxygen is radiated by external ultraviolet radiation to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is regulated to be 1:0.015, and the other conditions are the same to obtain electrolyte S2;

[0085] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S2 is 0.018 mol / L;

[0086] In step (4), the electrolyte S2 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q2 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0087] Example 3

[0088] According to the method of Example 1, the difference is that

[0089] In step (3), the ultraviolet wavelength is controlled to be 100 nm, and the irradiation is carried out at a power of 600 W for 1 hour, so that the remaining dissolved oxygen is irradiated with external ultraviolet light to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is regulated to be 1:0.03, and the other conditions are the same to obtain electrolyte S3;

[0090] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S3 is 0.024 mol / L;

[0091] In step (4), the electrolyte S3 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q3 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0092] Example 4

[0093] According to the method of Example 1, the difference is that

[0094] In step (3), the ultraviolet wavelength is controlled to be 180nm, and the radiation is carried out at a power of 800W for 0.5h, so that the remaining dissolved oxygen is radiated by external ultraviolet radiation to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is regulated to be 1:0.05, and the other conditions are the same to obtain electrolyte S4;

[0095] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S4 is 0.03 mol / L;

[0096] In step (4), the electrolyte S4 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q4 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0097] Example 5

[0098] According to the method of Example 1, the difference is that

[0099] In step (3), the ultraviolet wavelength is controlled to be 320nm, and the radiation is carried out at a power of 300W for 0.5h, so that the remaining dissolved oxygen is radiated by external ultraviolet radiation to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is adjusted to be 1:0.008. The other conditions are the same to obtain electrolyte S5.

[0100] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S5 is 0.01 mol / L;

[0101] In step (4), the electrolyte S5 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q5 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0102] Example 6

[0103] According to the method of Example 1, the difference is that

[0104] In step (3), the ultraviolet wavelength is controlled to 160nm, and the radiation is carried out at a power of 400W for 6 hours, so that the remaining dissolved oxygen is radiated by external ultraviolet radiation to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is adjusted to 1:0.8. The other conditions are the same to obtain electrolyte S6.

[0105] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S6 is 0.052 mol / L;

[0106] In step (4), the electrolyte S6 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q6 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0107] Example 7

[0108] According to the method of Example 1, the difference is that

[0109] In step (3), the ultraviolet wavelength is controlled to be 160nm, and the radiation is carried out at a power of 800W for 12h, so that the remaining dissolved oxygen is radiated by external ultraviolet radiation to obtain ozone, and the molar ratio of oxygen and ozone in the dissolved oxygen is adjusted to be 1:2. The other conditions are the same to obtain electrolyte S7.

[0110] Wherein, the concentration of dissolved oxygen in the above electrolyte liquid S7 is 0.076 mol / L;

[0111] In step (4), the electrolyte S7 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q7 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0112] Example 8

[0113] According to the method of Example 1, the difference is that

[0114] There is no step (3), and the mixed solution obtained in step (2) is directly used as the electrolyte S8;

[0115] In step (4), the electrolyte S8 is injected into the lithium ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium ion battery Q8 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0116] Comparative Example 1

[0117] According to the method of Example 1, the difference is that

[0118] Without steps (2)-(3), the mixed solution obtained in step (1) is directly used as the electrolyte DS1;

[0119] In step (4), the electrolyte DS1 is injected into the lithium-ion battery P1, and after being fully infiltrated, it is formed at 25±5°C, and then sealed after exhausting, filling, charging, aging, capacity separation, and self-discharge detection. The finished lithium-ion battery DQ1 is tested for discharge capacity at different temperatures, and the test results are listed in Table 1.

[0120] Table 1

[0121]

[0122] Table 1

[0123]

[0124] It can be seen from the data in Table 1 that, compared with Comparative Example 1, the finished lithium-ion batteries obtained by injecting the electrolytes prepared in Examples 1-8 into lithium-ion batteries have higher capacity retention rates at low temperatures and higher cycle capacity retention rates.

[0125] The photoelectron spectroscopy (XPS) spectra of the SEI film of the finished lithium ion battery containing the electrolyte of Example 1 and Comparative Example 1 are as follows: Figure 1 and Figure 2 As shown by Figure 1-2 It can be seen that compared with Comparative Example 1, the Li2O content in the SEI structure of the finished lithium-ion battery Q1 containing the electrolyte S1 of Example 1 is higher.

[0126] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte contains dissolved oxygen, lithium salt and organic solvent; wherein the dissolved oxygen includes oxygen.

2. The electrolyte according to claim 1, characterized in that The concentration of dissolved oxygen in the electrolyte is 0.001-0.1 mol / L, preferably 0.005-0.05 mol / L.

3. The electrolyte according to claim 1 or 2, characterized in that The dissolved oxygen also includes ozone; Preferably, the ozone in the dissolved oxygen is obtained by subjecting the dissolved oxygen to ultraviolet radiation.

4. The electrolyte according to claim 3, characterized in that In the dissolved oxygen, the molar ratio of oxygen to ozone is 1:0.001-1, preferably 1:0.005-0.1, and more preferably 1:0.01-0.

1.

5. The electrolyte according to claim 3, characterized in that The conditions of the ultraviolet radiation include: the ultraviolet wavelength is 10-400nm, preferably 100-400nm; the power of the ultraviolet generator is 10-3000W, preferably 60-600W; the ultraviolet radiation time is 0.1-1000min, preferably 1-100min.

6. The electrolyte according to any one of claims 1 to 5, characterized in that The concentration of the lithium salt in the electrolyte is 5-30wt%, preferably 7-20wt%; And / or, the lithium salt is selected from at least one of LiPF6, LiAsF6, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide and their derivatives; And / or, the organic solvent is selected from at least one of ether compounds, ester compounds, amide compounds, nitrile compounds and aromatic compounds, preferably selected from ether compounds and / or ester compounds.

7. The electrolyte according to any one of claims 1 to 6, characterized in that The electrolyte further includes an additive; Preferably, the content of the additive in the electrolyte is 0.05-10wt%, preferably 0.1-5wt%; Preferably, the additive is selected from at least one of vinylene carbonate, fluoroethylene carbonate, lithium difluorophosphate, lithium dioxalatoborate, lithium difluorooxalatoborate, 1,3-propane sultone, triallyl isocyanurate, methylene methanedisulfonate, vinyl sulfate, triallyl phosphate and tripropynyl phosphate.

8. A lithium ion battery, characterized in that: The lithium-ion battery comprises: a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte according to any one of claims 1 to 7.

9. The lithium-ion battery according to claim 8, characterized in that: The lithium-ion battery is subjected to formation to form a SEI film on the surface of the negative electrode plate; Preferably, the formation temperature is 20-40°C, preferably 20-30°C.

10. The lithium ion battery according to claim 9, characterized in that: The SEI film contains Li2O; based on the total weight of the SEI film, the content of Li2O is 10-40wt%, preferably 15-35wt%; Preferably, the SEI film further contains Li2CO3; based on the total weight of the SEI film, the content of Li2CO3 is 40-80wt%, preferably 50-70wt%; Preferably, the thickness of the SEI film is 2-200 nm, preferably 10-100 nm.

11. The lithium ion battery according to any one of claims 8 to 10, characterized in that: The charge transfer impedance of the lithium ion battery at -20°C is ≤1.2Ω·Ah, preferably 0.1-0.5Ω·Ah; And / or, the capacity retention rate of the lithium ion battery at -20°C is ≥65%, preferably 65-80%; the capacity retention rate after 500 cycles at 25°C is ≥91%, preferably 93.5-97.5%.

12. An electrical device, characterized in that: The electrical equipment comprises the lithium-ion battery according to any one of claims 8 to 11.

Citation Information

Patent Citations

  • Ultralow-temperature lithium ion battery electrolyte

    CN113036223A

  • Flame-retardant electrolyte and preparation method and application thereof

    CN115911552A

  • Production of nickel oxyhydroxide and nonaqueous electrolytic battery

    JP1998316432A

  • Organic electrolyte liquid for lithium second battery and lithium second battery thereof

    KR1020000003217A