A mesoporous solar cell and a method for preparing the same

By using porous metal layer and modification layer in mesoporous solar cells, the problems of large contact resistance and low carrier mobility in mesoporous solar cells are solved, and efficient photoelectric conversion and low internal resistance are achieved.

CN118870840BActive Publication Date: 2024-11-22旗滨新能源发展(深圳)有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411367552.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

In mesoporous solar cells, due to the large contact resistance between semiconductor metal oxides and conductive substrates and low carrier mobility, the photoelectric conversion efficiency is affected.

Method used

A porous metal layer is prepared on a conductive substrate, and a dense modification layer is formed on its surface to reduce contact resistance, fill with photosensitive materials to improve carrier collection efficiency, and form a metal-semiconductor/insulator-semiconductor structure.

Benefits of technology

Through the design of the ohmic contact and modification layer, the contact resistance between the mesoporous metal layer and the conductive substrate is reduced, the carrier collection area is increased, the photoelectric conversion efficiency is improved, and the internal resistance is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118870840B_ABST
    Figure CN118870840B_ABST
Patent Text Reader

Abstract

The present invention discloses a mesoporous solar cell and a preparation method thereof, and relates to the technical field of solar cells. The mesoporous solar cell comprises a conductive substrate, and a mesoporous metal layer and an electrode layer sequentially arranged on the conductive substrate; wherein the mesoporous metal layer comprises a porous metal and a modified layer attached to the surface of the porous metal; the conductive substrate is in contact with the porous metal; wherein the modified layer comprises at least one of a metal oxide, a metal nitride and an epoxy resin; at least the pores of the porous metal are filled with a photosensitizing material. In the present invention, an ohmic contact is formed between the porous metal and the conductive substrate to reduce the contact resistance, and the modified layer can block the direct contact between the porous metal and the photosensitizing material, play a charge blocking role, and inhibit the recombination of electrons and holes at the interface of the photosensitizing material and the porous metal. Therefore, the mesoporous solar cell provided by the present invention has the technical effect of low internal resistance and high photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a mesoporous solar cell and a preparation method thereof. Background Art

[0002] In mesoporous solar cells, the electron transport material or hole transport material of the mesoporous structure is based on semiconductor metal oxide materials such as mesoporous titanium oxide or tin oxide, nickel oxide, etc., which have poor conductivity. The semiconductor band bending is easy to occur at the contact interface between the semiconductor metal oxide and the conductive substrate, resulting in the formation of a contact barrier and thus increasing the contact resistance. Therefore, the contact resistance between the semiconductor metal oxide and the conductive substrate is relatively large.

[0003] In addition, carriers migrate and diffuse in mesoporous semiconductor metal oxides under the action of concentration gradient and built-in electric field until they reach the conductive substrate and are collected. Due to the low mobility and high resistance of carriers in oxides, electron-hole recombination occurs during the migration process, resulting in low carrier collection efficiency, which in turn affects the photoelectric conversion efficiency. Summary of the invention

[0004] The main purpose of the present invention is to provide a mesoporous solar cell and a preparation method thereof, aiming to solve the problems of large internal resistance and low carrier mobility of existing mesoporous solar cells.

[0005] To achieve the above-mentioned purpose, the present invention proposes a mesoporous solar cell, which includes a conductive substrate, and a mesoporous metal layer and an electrode layer sequentially arranged on the conductive substrate; wherein the mesoporous metal layer includes a porous metal and a modified layer attached to the surface of the porous metal; the conductive substrate is in contact with the porous metal; the modified layer includes at least one of metal oxide, metal nitride and epoxy resin; at least the pores of the porous metal are filled with photosensitizing material.

[0006] In one embodiment, the porous metal material includes at least one of titanium, nickel, aluminum, manganese, tin, niobium, tantalum, copper, cobalt, indium, and tungsten.

[0007] In one embodiment, the metal oxide includes at least one of titanium dioxide, aluminum oxide, nickel dioxide and magnesium oxide; and / or,

[0008] The metal nitride includes at least one of aluminum nitride, gallium nitride and indium nitride.

[0009] In one embodiment, the thickness of the mesoporous metal layer is 100 nm to 1000 nm; and / or,

[0010] The pore size of the porous metal is 10nm~1000nm; and / or,

[0011] The thickness of the modified layer is 0.1 nm to 4 nm.

[0012] In one embodiment, a mesoporous insulating spacer layer is further disposed between the mesoporous metal layer and the electrode layer.

[0013] In one embodiment, the photosensitizing material includes at least one of a perovskite material and a photosensitizing dye.

[0014] The present invention also provides a method for preparing the mesoporous solar cell as described above, comprising the following steps:

[0015] preparing porous metal on a conductive substrate;

[0016] preparing a modified layer on the surface of the porous metal to obtain a mesoporous metal layer;

[0017] At least an electrode layer is prepared on the surface of the mesoporous metal layer to obtain a mesoporous solar cell;

[0018] Wherein, at least the pores of the mesoporous metal layer are filled with photosensitizing material.

[0019] In one embodiment, the step of preparing a porous metal on a conductive substrate comprises:

[0020] The nano-metal is mixed with ethyl cellulose, pine alcohol, ethanol and citric acid, ball-milled, and distilled under reduced pressure to obtain a metal slurry;

[0021] The metal slurry is deposited on a conductive substrate and sintered in a reducing atmosphere to prepare a porous metal.

[0022] In one embodiment, in the step of depositing the metal slurry on the conductive substrate and sintering in a reducing atmosphere to prepare the porous metal, the sintering temperature is 300-550°C.

[0023] In one embodiment, in the step of mixing the nano metal with ethyl cellulose, terpineol, ethanol and citric acid, ball milling, and distilling under reduced pressure to obtain the metal slurry:

[0024] The mass ratio of the nano metal, ethyl cellulose, pinene alcohol, ethanol and citric acid is (1-2): 1: (7-10): (30-50): (0.001-0.01); and / or,

[0025] The ball milling time is 8 to 20 hours; and / or,

[0026] The temperature of the reduced pressure distillation is 40-50°C; and / or,

[0027] The pressure of the reduced pressure distillation is 0.01-0.02 MPa; and / or,

[0028] The particle size of the nano metal is 20-200 nm.

[0029] In the technical solution of the present invention, the structure prepares a three-dimensional conductive porous metal on a conductive substrate, and the porous metal is directly connected to the conductive substrate, so that an ohmic contact is formed between the metal and the conductive substrate to reduce the contact resistance. However, since the photosensitizer is corrosive to the metal, a dense modification layer is formed on the surface of the porous metal as a barrier to achieve surface modification of the porous metal and avoid reaction between the photosensitizer and the metal. A metal / modified layer composite structure, i.e., a mesoporous metal layer, is obtained by forming a continuous and dense modified layer on the surface of the porous metal; the mesoporous structure in the mesoporous metal layer provides a space for filling the photosensitizer material, and the thinner modified layer on the surface of the porous metal is between the photosensitizer material and the porous metal, acting as a charge blocking layer to inhibit the recombination of electrons and holes at the interface between the photosensitizer material and the porous metal; in the mesoporous metal layer, a modified layer is added between the porous metal and the semiconductor of the photosensitizer material to improve the electrical properties, and the porous metal, the dense modified layer and the photosensitizer material together form a metal-semiconductor / insulator (modified layer)-semiconductor (photosensitizer material) structure, which can reduce the contact resistance between the mesoporous metal layer and the conductive substrate. In addition, due to the large specific surface area of ​​the porous metal and the ohmic contact formed with the conductive substrate, the effective area of ​​the conductive substrate for collecting carriers is greatly increased, and the carriers can pass through the modified layer and be collected by the porous metal in a very short time, which promotes the separation of charges at the interface of the porous metal and the perovskite and prevents the accumulation of carriers at the interface. Therefore, the mesoporous solar cell provided by the present invention has the technical effects of low internal resistance and high photoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0031] Figure 1 A schematic structural diagram of an embodiment of a mesoporous solar cell proposed by the present invention;

[0032] Figure 2 This is a schematic diagram of the structure of a mesoporous metal layer of a mesoporous solar cell in one embodiment of the present invention;

[0033] Figure 3 A schematic diagram of the structure of a mesoporous metal layer of a mesoporous solar cell in another embodiment of the present invention;

[0034] Figure 4 This is an IV curve diagram of the mesoporous solar cell obtained in Example 1 of the present invention;

[0035] Figure 5 This is an IV curve diagram of the mesoporous solar cell obtained in Example 2 of the present invention;

[0036] Figure 6 This is an IV curve diagram of the mesoporous solar cell obtained in Example 3 of the present invention;

[0037] Figure 7 This is an IV curve diagram of the mesoporous solar cell obtained in Example 4 of the present invention;

[0038] Figure 8 This is an IV curve diagram of the mesoporous solar cell obtained in Example 5 of the present invention;

[0039] Fig. 9 This is an IV curve diagram of the mesoporous solar cell obtained in Example 6 of the present invention;

[0040] Fig.10 The IV curves of the mesoporous solar cells obtained in Example 7 of the present invention and Comparative Example 2;

[0041] Fig.11 This is an IV curve diagram of the mesoporous solar cell obtained in Example 8 of the present invention;

[0042] Fig.12 This is an IV curve diagram of the mesoporous solar cell obtained in Example 9 of the present invention;

[0043] Fig.13 This is an IV curve diagram of the mesoporous solar cell obtained in Comparative Example 1 of the present invention;

[0044] Fig.14 This is an IV curve diagram of the mesoporous solar cell obtained in Comparative Example 3 of the present invention.

[0045] Description of Figure Numbers:

[0046] 100. Mesoporous solar cell; 1. Conductive substrate; 2. Mesoporous metal layer; 21. Porous metal; 22. Modification layer; 3. Electrode layer; 4. Mesoporous insulating spacer layer.

[0047] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0050] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the "and / or" or "and / or" appearing in the full text include three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0051] In mesoporous solar cells, the electron transport material or hole transport material of the mesoporous structure is based on semiconductor metal oxide materials such as mesoporous titanium oxide or tin oxide, which have poor intrinsic conductivity. However, the semiconductor band bending is prone to occur at the contact interface between the semiconductor metal oxide and the conductive substrate, resulting in the formation of a contact barrier and thus increasing the contact resistance. Therefore, the contact resistance between the semiconductor metal oxide and the conductive substrate is relatively large.

[0052] In addition, carriers migrate and diffuse in mesoporous semiconductor metal oxides under the action of concentration gradient and built-in electric field until they reach the conductive substrate and are collected. Due to the low mobility and high resistance of carriers in oxides, electron-hole recombination occurs during the migration process, resulting in low carrier collection efficiency, which in turn affects the photoelectric conversion efficiency.

[0053] The bending of the metal and semiconductor interface band depends on the work function of the metal and the Fermi level of the semiconductor. When the metal electrode work function is higher than the N-type semiconductor work function or the metal electrode work function is lower than the P-type semiconductor work function, a Schottky barrier is formed at the semiconductor and metal interface. Compared with the PN junction, the diode based on the Schottky barrier has a large leakage current and a low forward conduction voltage, and is less efficient when used in photovoltaic devices.

[0054] In view of this, the present invention proposes a mesoporous solar cell 100, see Figure 1 and Figure 2 The mesoporous solar cell 100 includes a conductive substrate 1, and a mesoporous metal layer 2 and an electrode layer 3 sequentially arranged on the conductive substrate 1; wherein the mesoporous metal layer 2 includes a porous metal 21 and a modified layer 22 attached to the surface of the porous metal 21; the conductive substrate 1 is in contact with the porous metal 21, and the modified layer 22 covers the exposed surfaces of the conductive substrate 1 and the porous metal 21; at least the pores of the porous metal 21 are filled with photosensitizing material.

[0055] In the technical solution of the present invention, the structure is prepared by preparing a three-dimensional conductive porous metal 21 on a conductive substrate 1, and the porous metal 21 is directly connected to the conductive substrate 1, so that an ohmic contact is formed between the metal and the conductive substrate 1 to reduce the contact resistance. However, since the photosensitizing material is corrosive to the metal, a dense modification layer 22 is formed on the surface of the porous metal 21 as a barrier to achieve surface modification of the porous metal 21 and avoid the reaction between the photosensitizing material and the metal. By forming a continuous and dense modification layer 22 on the surface of the porous metal 21, a metal / modification layer 22 composite structure, that is, a mesoporous metal layer 2, is obtained; the mesoporous structure in the mesoporous metal layer 2 provides a space that can be filled with the photosensitizing material, and the thinner modification layer 22 on the surface of the porous metal 21 is between the photosensitizing material and the porous metal 21, and acts as a charge blocking layer to inhibit the recombination of electrons and holes at the interface between the photosensitizing material and the porous metal 21; in the mesoporous metal layer 2, a modification layer 22 is added between the porous metal 21 and the semiconductor of the photosensitizing material to improve the electrical properties, and the porous metal The metal-semiconductor / insulator (modified layer 22)-semiconductor (photosensitized material) structure is formed by the metal 21, the dense modified layer 22 and the photosensitizing material, which can reduce the contact resistance between the mesoporous metal layer 2 and the conductive substrate 1. In addition, due to the large specific surface area of ​​the porous metal 21 and the ohmic contact with the conductive substrate 1, the effective area of ​​the conductive substrate 1 for collecting carriers is greatly increased. The carriers can pass through the modified layer 22 in a very short time and be collected by the porous metal 21, which promotes the separation of charges at the interface between the porous metal 21 and the perovskite and prevents the accumulation of carriers at the interface. Therefore, the mesoporous solar cell 100 provided by the present invention has the technical effects of low internal resistance and high photoelectric conversion efficiency.

[0056] See also Figure 2 It should be noted that the porous metal 21 refers to a metal substance with nano-scale pores inside, and the surface of the porous metal 21 refers to the outer surface and pore surface of the porous metal 21; the modified layer 22 covers the surface of the porous metal 21 that is not in contact with the conductive substrate 1, that is, there is no modified layer 22 blocking the porous metal 21 and the conductive substrate 1 (contact site), the porous metal 21 is in direct contact with the conductive substrate, and there is a modified layer 22 between the porous metal 21 and other external environments or photosensitizing materials to block the porous metal 21 from other external environments or photosensitizing materials. The photosensitizing material is also called a photoactive material, which refers to a material that can generate photoelectrons under light conditions, such as metal halide perovskite materials, quantum dots, and photosensitizing dyes.

[0057] In some embodiments, the modification layer 22 also covers the exposed portion of the conductive substrate 1 , that is, the conductive substrate 1 and the porous metal 21 can be understood as a partially contacting whole, and the surface of the whole is covered by the modification layer 22 .

[0058] It is understandable that the structure can be implemented in the following ways:

[0059] The porous metal 21 is prepared on the conductive substrate 1 to obtain the porous metal 21 material, and the position where the porous metal 21 contacts the conductive substrate is inside the entire porous metal 21 material. Therefore, when the modification layer 22 is prepared on the surface of the porous metal 21 material, the surface of the porous metal 21 material is covered by the modification layer 22, that is, the part of the porous metal 21 that is not in contact with the conductive substrate will be covered by the modification layer 22. In this way, the porous metal 21 can directly contact the conductive substrate 1, but will not directly contact the material filled in the pores or the external environment due to the modification layer 22.

[0060] The material of the porous metal 21 can be a transition metal, or a non-transition metal that is relatively stable under normal conditions, or an alloy material obtained from the above metals. Furthermore, the material of the porous metal 21 includes at least one of titanium, nickel, aluminum, manganese, tin, niobium, tantalum, copper, cobalt, indium, and tungsten. The above metal materials have good electrical conductivity and electron mobility. The use of the above metal materials can effectively transfer photogenerated electrons from the perovskite absorption layer to the electrode, reduce the loss of electrons during the transmission process, and thus improve the photoelectric conversion efficiency of the battery. In addition, without paying attention to cost, the material of the porous metal 21 can also be rare precious metals such as gold, platinum, and silver.

[0061] Furthermore, the metal oxide includes at least one of titanium dioxide, aluminum oxide, nickel dioxide and magnesium oxide. The metal oxide has a wide band gap, can transmit visible light, and can well block the recombination of electron holes at the interface of the electrode and the perovskite, and the metal oxide has good chemical stability, which can effectively improve the photoelectric conversion efficiency and stability of the battery.

[0062] Furthermore, the metal nitride includes at least one of aluminum nitride, gallium nitride and indium nitride. The above nitride can effectively block the recombination of electron holes at the interface between the electrode and the perovskite, and the above metal nitride has good photoelectric properties and chemical stability, and can effectively improve the photoelectric conversion efficiency and stability of the battery.

[0063] It is understandable that oxides or nitrides of titanium, aluminum, manganese, tin, niobium, tantalum, copper, cobalt, indium, and tungsten can also be used as the material of the modification layer 22. The present invention is not limited to using only at least one of titanium dioxide, aluminum oxide, nickel oxide, magnesium oxide, aluminum nitride, gallium nitride, and indium nitride.

[0064] In the mesoporous solar cell 100, the thickness of the mesoporous metal layer 2 is 100nm~1000nm, specifically, the thickness of the mesoporous metal layer 2 can be 100nm, 150nm, 200nm, 400nm, 1000nm, etc. The thickness of the mesoporous metal layer 2 is less than 100nm, which will limit the filling of the perovskite and the contact area between the perovskite and the electrode, and the thinner mesoporous metal layer 2 is difficult to fully absorb and utilize the energy in the solar cell, resulting in partial energy loss during transmission, thereby affecting the photoelectric conversion efficiency of the battery and reducing its output power. When the thickness of the mesoporous metal layer 2 is higher than 1000nm, due to the enhanced reflection effect of light, the incident light reaching the photosensitive layer will be reduced to a certain extent, resulting in a decrease in light transmittance.

[0065] The porous metal 21 and the modified layer 22 on the surface of the porous metal 21 together constitute the mesoporous metal layer 2, and the porous metal 21 has nanoscale pores inside, and the pore size of the porous metal 21 is 10nm~1000nm, for the coating of the modifier and the filling of the perovskite. If the pore size is too small, the perovskite is not easy to fill the pores, and the pore size limits the perovskite grain size. The smaller perovskite has more defects, and the pore size is too small, the light transmittance decreases, and the perovskite receives insufficient light, resulting in lower current density and performance. The pore size is too large, the metal electrode is less connected, the square resistance reduction effect is not obvious, and the strength of the mesoporous metal is also reduced accordingly. Preferably, the pore size of the porous metal 21 is 10nm~500nm. It should be noted that the pore size of the porous metal 21 should be smaller than the thickness of the mesoporous metal layer 2.

[0066] The thickness of the modified layer 22 is 0.1nm~4nm. The modifier is between the photosensitizing material and the metal electrode, and has the function of blocking electrons or holes to inhibit the recombination of electrons and holes at the interface of the photosensitizing material and the metal electrode; at the same time, the thin layer of the modified layer 22 can enable the carriers to quickly pass through the modified layer 22 from the photosensitizing material to the porous metal 21, promote the separation of charges at the interface of the porous metal 21 and the perovskite, and prevent the accumulation of carriers at the interface. Therefore, if the thickness of the modified layer 22 is too thick, the migration resistance of the carriers will increase, and there will be a reflective effect of the grain boundary, which will reduce the transparency. If the thickness of the modified layer 22 is too thin, especially when the modified layer 22 obtained by the metal oxide or nitride is too thin, it may cause the metal substance to be unable to be completely coated, thereby causing corrosion reaction or recombination of carriers. Therefore, the thickness of the modified layer 22 is 0.1nm~4nm, which can not only better isolate the porous metal 21 from the photosensitizing material, but also reduce the migration resistance of the carriers.

[0067] It should be noted that the thickness of the mesoporous metal layer 2 is 100nm~1000nm, the pore size of the porous metal 21 is 10nm~500nm, and the thickness of the modified layer 22 is 0.1nm~4nm. The above three can be set simultaneously or separately. When set separately, it should be considered that the pore size of the porous metal 21 must be greater than twice the thickness of the modified layer 22, otherwise the modified layer 22 will block the pores of the porous metal 21 and cannot accommodate the photosensitized material. When the three are set simultaneously, a better photoelectric conversion effect can be obtained.

[0068] In addition, other structures may be arranged between the mesoporous metal layer 2 and the electrode layer 3 according to specific application scenarios or requirements. Figure 1 and Figure 3 In the mesoporous solar cell 100, a mesoporous insulating spacer layer 4 is also provided between the mesoporous metal layer 2 and the electrode layer 3. The mesoporous insulating spacer layer 4 is provided to avoid direct contact between the mesoporous metal layer 2 and the electrode layer 3, and to prevent serious electron-hole recombination. The mesoporous structure of the mesoporous insulating spacer layer 4 not only provides support and attachment points for the growth of the perovskite material, which contributes to the uniform distribution and stable existence of the perovskite layer, but also can affect the propagation path of sunlight in the battery, increase the propagation length of light in the battery, and thus improve the absorption efficiency of perovskite to light. It should be noted that when the mesoporous solar cell 100 does not contain a mesoporous insulating layer, the electrode layer 3 should be at a certain distance from the porous metal 21 in the mesoporous metal layer 2, and can be separated by the perovskite, or by a modification layer 22 of a few nanometers.

[0069] The photosensitizing material includes at least one of a perovskite material and a photosensitizing dye. In the technical solution of the present application, the perovskite material can be filled in the pores of the porous metal 21 to obtain a mesoporous perovskite solar cell, and the photosensitizing dye can be adsorbed on the surface of the modified layer 22 to obtain a dye-sensitized solar cell. The mesoporous solar cell 100 of the above structure is widely used and has a high photoelectric conversion efficiency.

[0070] It should be noted that, in the actual manufacturing process, not only the mesoporous metal layer 2 is filled with the photosensitizing material, but also when the electrode layer 3 has a mesoporous structure, the electrode layer 3 can be filled with photosensitizing material, and when a mesoporous insulating spacer layer 4 is provided between the mesoporous metal layer 2 and the electrode layer 3, the electrode layer 3, the mesoporous insulating spacer layer 4 and the mesoporous metal layer 2 are all filled with photosensitizing material to form a mesoporous solar cell 100. In addition, the material of the electrode layer 3 can be one of carbon, titanium and nickel. It can also be other commonly used conductive electrode materials, which are not limited here and can be selected according to needs.

[0071] The present invention further provides a method for preparing the mesoporous solar cell 100 as described above, and the method for preparing the mesoporous solar cell 100 comprises the following steps:

[0072] Preparing a porous metal 21 on a conductive substrate 1;

[0073] Prepare a modified layer 22 on the surface of the porous metal 21 to obtain a mesoporous metal layer 2;

[0074] At least an electrode layer 3 is prepared on the surface of the mesoporous metal layer 2 to obtain a mesoporous solar cell 100;

[0075] Wherein, at least the pores of the mesoporous metal layer 2 are filled with photosensitizing material.

[0076] It should be noted that the electrode layer 3 can be directly prepared on the surface of the mesoporous metal layer 2 to obtain the mesoporous solar cell 100, and other layers can also be prepared on the surface of the mesoporous metal layer 2 as needed. In some embodiments, a mesoporous insulating spacer layer 4 is prepared on the surface of the mesoporous metal layer 2, and an electrode layer 3 is prepared on the surface of the mesoporous insulating spacer layer 4 to obtain the mesoporous solar cell 100.

[0077] It is understandable that the filling of the photosensitizing material can be done after preparing the electrode layer 3 or before preparing the electrode layer 3. Taking the preparation of the electrode layer 3 directly on the surface of the mesoporous metal layer 2 as an example, the electrode layer 3 can be prepared on the surface of the mesoporous metal layer 2 first, and then the photosensitizing material is filled from the surface of the electrode layer 3 to the mesoporous metal layer 2 to complete the preparation of the mesoporous solar cell 100. In this case, it is understandable that the electrode layer 3 has a mesoporous structure so that the photosensitizing material can pass through the electrode layer prepared with the mesoporous material to reach the pores of the mesoporous metal layer 2; the photosensitizing material can also be directly filled into the mesoporous metal layer 2, and then the electrode layer 3 is prepared on the surface of the mesoporous metal layer 2 filled with the photosensitizing material to obtain the mesoporous solar cell 100. In this case, the electrode layer 3 can have a mesoporous structure or not.

[0078] In some embodiments, the modification layer 22 covers both the bare metal and the conductive substrate 1 that is not in contact with the metal, that is, a modification layer 22 is also formed on the bare conductive substrate 1 that is not covered by the metal.

[0079] The steps of preparing the porous metal 21 on the conductive substrate 1 include: mixing the nano metal with ethyl cellulose, pine alcohol, ethanol and citric acid, ball milling, and distilling under reduced pressure to obtain metal slurry; depositing the metal slurry on the conductive substrate 1, and sintering in a reducing atmosphere to prepare the porous metal 21. Before depositing the metal slurry on the conductive substrate 1, the corresponding metal slurry is prepared according to the type and characteristics of the selected metal.

[0080] The mass ratio of the nano metal, ethyl cellulose, pine alcohol, ethanol and citric acid is (1-2): 1: (7-10): (30-50): (0.001-0.01). Specifically, the mass ratio of the nano metal, ethyl cellulose, pine alcohol, ethanol and citric acid can be 1: 1: 7: 50: 0.01 or 2: 1: 10: 40: 0.005 or 1.5: 1: 8: 40: 0.001, etc. The appropriate amount of citric acid added can improve the surface tension and wettability of the metal slurry, making it easier to obtain a uniformly dispersed and stable slurry, thereby maintaining the stability and uniformity of the metal slurry so that the metal slurry can form a uniform, porous structure after sintering. As a dispersion carrier, pine alcohol and ethanol can dissolve citric acid, ethyl cellulose and other components to form a uniform slurry. The change in the amount of pine alcohol and ethanol added can also adjust the viscosity of the metal slurry, making it easier to operate and apply. The slurry with an appropriate viscosity can better form a uniform coating on the conductive substrate 1. Ethyl cellulose will burn or decompose during the sintering process to form pores between metal particles, thereby obtaining a porous metal 21 structure. Therefore, ethyl cellulose, as a pore-forming agent, can help nanometals form nanopores when preparing mesoporous metals.

[0081] By ball milling, the nano-metal particles can be evenly dispersed in the mixture of ethyl cellulose, pine alcohol, ethanol and citric acid, so that in the subsequent process, the metal particles can be evenly deposited on the conductive substrate 1 to form a uniform porous metal 21. The ball milling time is 8 to 20 hours, and specifically, the ball milling time can be 8 hours, 12 hours, 15 hours, and 20 hours. Too short a ball milling time will result in the nano-metal particles and additives such as ethyl cellulose, pine alcohol, ethanol and citric acid not being completely mixed evenly, and as the ball milling time increases, the mixing effect gradually increases, making the metal particles in the slurry more evenly distributed. In addition, during the ball milling process, the agglomerated large metal particles are continuously impacted and sheared under the action of the ball milling medium, thereby being refined. Therefore, increasing the ball milling time helps to obtain a smaller particle size and a more uniform particle distribution, which helps to improve the stability and coating performance of the slurry. And as the ball milling time increases, the viscosity of the slurry gradually decreases and the fluidity is better, which is convenient for subsequent coating or printing. However, too long a ball milling time may also lead to problems such as increased energy consumption, increased equipment wear and reduced production efficiency. Therefore, by mixing nanometal with ethyl cellulose, pinene alcohol, ethanol and citric acid and ball milling for 8 to 20 hours, a metal slurry with uniform mixing, fine particles, appropriate viscosity, good fluidity and good stability can be obtained.

[0082] In order to effectively distill and remove volatile solvents such as ethanol and pinene alcohol, while avoiding decomposition or reaction of substances caused by excessive temperature, in some embodiments, the temperature of the vacuum distillation is 40-50°C, specifically, the temperature of the vacuum distillation can be 40°C, 45°C, 50°C, etc. Vacuum distillation helps to accelerate the volatilization of the solvent and rapidly reduce the solvent content in the slurry, thereby obtaining a metal slurry with pinene alcohol as an organic carrier. Therefore, vacuum distillation at a temperature of 40-50°C can effectively remove low-boiling point solvents, retain organic additives and organic carriers, and control the viscosity of the slurry, thereby obtaining high-quality metal slurry.

[0083] During the vacuum distillation process, the pressure will also affect the effect of the vacuum distillation. Therefore, in some embodiments, the pressure of the vacuum distillation is 0.01~0.02MPa, specifically, the pressure of the vacuum distillation is 0.01MPa, 0.015MPa, 0.02MPa, etc. At a relatively low pressure of 0.01~0.02MPa, volatile solvents such as ethanol can be removed more quickly, while pine alcohol is not easy to volatilize and can be better retained in the slurry. Therefore, vacuum distillation at a pressure of 0.01~0.02MPa can accelerate the volatilization of low-boiling point solvents and retain designated organic components, thereby obtaining high-quality metal slurry.

[0084] Nanometal (also known as nanocrystalline metal or nanostructured metal) refers to metal materials with nano-scale grain size. Nanometal is a new type of structural metal material, and its microstructure is mainly composed of nano-scale grains and a large number of grain boundaries in three-dimensional space. In some embodiments, the particle size of the nanometal is 20-200nm, which makes it easier to achieve uniform dispersion of nanometal particles in the slurry, reduces the possibility of particle agglomeration and sedimentation, and improves the stability and coating performance of the slurry, so that nano-scale pores can be formed after sintering for perovskite filling.

[0085] After the metal slurry is prepared, the metal slurry is deposited on the conductive substrate 1 and sintered in a reducing atmosphere to prepare the porous metal 21 ; during sintering, the organic matter in the metal slurry decomposes to form a mesoporous structure, namely the porous metal 21 .

[0086] The reducing atmosphere may be at least one of a hydrogen atmosphere, a carbon monoxide atmosphere or an ammonia atmosphere, or may be other reducing atmospheres. Sintering in a reducing atmosphere can prevent the metal from being oxidized during the sintering process, while promoting the decomposition and volatilization of organic solvents and additives.

[0087] The appropriate sintering temperature can not only decompose and volatilize the organic solvent and organic matter in the metal slurry to form a mesoporous structure, but also promote the diffusion and bonding between the metal particles. Therefore, in the step of depositing the metal slurry on the conductive substrate 1 and sintering it in a reducing atmosphere to prepare the porous metal 21, the sintering temperature is 300°C to 550°C. Specifically, the sintering temperature can be 300°C, 350°C, 400°C, 550°C, etc. If the sintering temperature is too low, the connection between the metal particles will not be tight enough, and the pore structure will not be uniform or stable enough. If the sintering temperature is too high, the metal particles may be over-sintered, the particles may grow or agglomerate, and the pore structure may be compressed or disappear, thereby reducing the porosity. Therefore, the sintering temperature of 300°C to 550°C can not only obtain a uniform and stable pore structure, but also improve the connection strength between the metal particles, thereby enhancing the mechanical strength of the material.

[0088] It should be noted that the present invention is not limited to only using the above method to prepare the porous metal 21 on the conductive substrate 1, and other methods can also be used as long as the porous metal 21 with nanopores can be prepared.

[0089] For example, it can be obtained by electrochemical corrosion, such as cathode electrodeposition of a Ni-Cu alloy layer on a conductive substrate, and then dissolving the metallic copper by dealloying to obtain porous metallic nickel. Specifically, the conductive substrate is used as the working electrode, Pt and Ag / AgCl are used as the counter electrode and reference electrode, respectively, and the deposition solution is a mixed solution of 1.0 mol / L NiSO4, 0.05 mol / L CuSO4 and 0.5 mol / L H3BO3. During operation, the cleaned conductive substrate is treated with ultraviolet ozone (UVO) for 10 minutes, and then electrodeposited. The cathode electrodeposition is carried out at a constant potential of -0.8 V, and the deposition amount is 0.1-1C / cm 2 After cathode deposition, in the same three-electrode system, an anodic potential of 0.5 V was applied to dissolve metallic copper with a cutoff current density of 15.0 μA·cm -2 Through the aforementioned electrochemical process, a conductive substrate 1 prepared with porous metal nickel can be obtained. It should be noted that this application only uses porous metal nickel to illustrate the specific implementation of the method, and does not limit the method to only preparing porous nickel on the conductive substrate 1.

[0090] It can also be obtained by magnetron sputtering and dealloying. Specifically, the copper target, magnesium target and substrate can be installed on the magnetron sputtering equipment respectively, and the coating vacuum is 1~5 Pa. By keeping the turntable speed at a constant 5~20rpm, controlling the sputtering parameters of Ar flow rate 10~50sccm, power 30~100W, and sputtering time 20~60 min, an alloy film is obtained, wherein the composition ratio of the alloy can be controlled by the sputtering power ratio of the two targets, for example, the mass ratio of copper and magnesium can be (15:85)~(30:70), and the thickness is 400nm. Subsequently, at room temperature, the prepared alloy film is immersed in a 1.00mol / L HCl solution to corrode the sample. When no bubbles are generated on the surface of the sample, it is repeatedly washed with deionized water, and then placed in a drying oven for vacuum drying to avoid oxidation of the sample, to obtain a conductive substrate 1 prepared with porous copper. And so on.

[0091] Subsequently, a modification layer 22 is prepared on the surface of the porous metal 21 to obtain a mesoporous metal layer 2. The present invention does not limit the method of preparing the modification layer 22 on the surface of the porous metal 21. The surface of the porous metal 21 can be directly oxidized to form a corresponding metal oxide, or a material corresponding to the modification layer 22 can be separately prepared on the surface of the porous metal 21.

[0092] Specifically, a layer of mesoporous Ti slurry can be printed on the conductive substrate 1, and sintered at 400 degrees in a reducing atmosphere with a volume ratio of hydrogen to nitrogen of 1:4 to obtain mesoporous Ti in direct contact with the conductive substrate 1. The conductive substrate 1 prepared with mesoporous Ti is placed in a vacuum chamber, evacuated to 100Pa, and a mixture of chlorine and water vapor is introduced. After 3 to 10 seconds, it is evacuated to 100Pa again to complete a cycle. The chlorine gas-water vapor flow ratio is (1:0.5) to (1:2), and the cumulative reaction time is 10 to 50 seconds. After the reaction is completed, it is washed with anhydrous ethanol and sintered at 500°C to complete the preparation of the titanium oxide coating layer. The reaction principle is that chlorine and titanium form titanium tetrachloride, and titanium tetrachloride decomposes into titanium oxide when it encounters water and adheres to the porous titanium and FTO surfaces. This method is to directly generate titanium oxide by reacting titanium on the surface of porous titanium with oxides. The preparation method is simple and the materials used are simpler than those for preparing modified materials from scratch.

[0093] In addition, a modification material can be prepared on the surface of the porous metal 21. Specifically, the conductive substrate 1 made of porous copper is immersed in a 40 mM titanium tetrachloride aqueous solution and reacted at 70°C for 30 to 40 minutes to generate a layer of titanium oxide on the surface. The titanium oxide coating is obtained by sintering at 400°C on the surface of the porous copper.

[0094] It should be noted that the present invention is not limited to only using the above-mentioned method to prepare the modification layer 22 .

[0095] After the mesoporous metal layer 2 is prepared, at least an electrode layer 3 is prepared on the surface of the mesoporous metal layer 2; in some embodiments, the electrode layer 3 is prepared on the surface of the mesoporous metal layer 2 by screen printing, which facilitates the control of the thickness of the electrode layer 3 and makes the prepared electrode layer 3 more uniform.

[0096] In addition, other materials or structures may be prepared between the mesoporous metal layer 2 and the electrode layer 3 to achieve corresponding effects. In some embodiments, a mesoporous insulating spacer layer 4 is also prepared between the mesoporous metal layer 2 and the back electrode layer 3. The material of the mesoporous insulating spacer layer 4 includes at least one of zirconium oxide and aluminum oxide, or other oxides. In specific operations, the mesoporous insulating spacer layer 4 may be prepared by screen printing.

[0097] Optionally, during the preparation process or after the electrode layer 3 is prepared, the photosensitizing material can be filled into at least the mesoporous metal layer 2 to obtain the mesoporous solar cell 100. When the electrode layer 3 is a mesoporous structure, when a mesoporous insulating spacer layer 4 is also provided between the mesoporous metal layer 2 and the electrode layer 3, the electrode layer 3, the mesoporous insulating spacer layer 4 and the mesoporous metal layer 2 are all filled with photosensitizing material to form the mesoporous solar cell 100 together.

[0098] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0099] Example 1

[0100] Provided is a mesoporous solar cell, which includes, arranged from bottom to top in sequence, a conductive substrate (FTO conductive glass), a 150nm thick mesoporous metal layer (including porous titanium and a 1nm thick titanium oxide coating layer), a 1μm thick mesoporous insulating spacer layer (mesoporous zirconia), and a 10μm thick electrode layer (mesoporous carbon), wherein the mesoporous metal layer, the mesoporous insulating spacer layer, and the electrode layer are all filled with perovskite.

[0101] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0102] Nano-titanium was mixed with ethyl cellulose, pinene alcohol, ethanol and citric acid in a mass ratio of 1:1:7:50:0.01, and ball-milled at a speed of 300 rpm for 20 h. After ball-milling, the mixture was rotary evaporated at 40°C and 0.01 MPa for 20 h to obtain nano-Ti slurry.

[0103] A layer of nano-Ti slurry was printed on the FTO conductive glass, and sintered at 400°C for 20 min in a reducing atmosphere (hydrogen to nitrogen volume ratio of 1:4) to obtain porous titanium in direct contact with the FTO conductive glass.

[0104] The square resistance of the FTO conductive glass prepared with porous titanium in this embodiment was tested using an FT-331 ordinary four-probe square resistance resistivity tester (Ningbo Ruike Micro Intelligent Technology Co., Ltd.) in a nitrogen-filled glove box. The electrode resistance of the deposited porous metal was significantly lower than that of the FTO substrate. The test data is shown in Table 1 Example 1.

[0105] The FTO conductive glass prepared with porous titanium was placed in a vacuum chamber, evacuated to 100Pa, and a mixture of chlorine and water vapor was introduced. After 6 seconds, the vacuum was evacuated to 100Pa again to complete a cycle. The chlorine gas and water vapor flow rate ratio was 1:1, and the above cycles were completed for 5 times to complete the reaction. After the reaction, it was washed with anhydrous ethanol and sintered at 500°C to obtain FTO conductive glass prepared with a porous Ti / titanium oxide layer (mesoporous metal layer);

[0106] A 1 μm thick layer of mesoporous zirconia slurry is screen-printed on the porous Ti / titanium oxide layer, and a 10 μm thick layer of mesoporous carbon slurry is printed after drying. After sintering at 400°C, the electrode layer, mesoporous insulating spacer layer and mesoporous metal layer are filled with perovskite solution, and crystallized at 57°C for 20 hours to obtain a mesoporous perovskite solar cell.

[0107] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Figure 4 As shown, the key electrical parameters are summarized in Example 1 in Table 2, where FF is higher and Rs is lower, indicating that the battery performance is better and the internal resistance is lower.

[0108] Example 2

[0109] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a 150nm thick mesoporous metal layer (including porous titanium and a 2nm aluminum oxide coating layer), and a 10μm thick electrode layer (mesoporous carbon) which are arranged in sequence from bottom to top, wherein the mesoporous metal layer and the electrode layer are both filled with perovskite.

[0110] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0111] Nano-titanium, citric acid, stabilizer (tetraoctylammonium bromide), and isopropanol were mixed in a mass ratio of 1:0.3:0.01:100, stirred and ultrasonically dispersed at -5°C to obtain a nano-titanium dispersion with a concentration of 0.01 mg / ml;

[0112] Spin-coat the nano-titanium dispersion on the FTO conductive glass at a speed of 3000 rpm / min to a thickness of about 40 nm, dry it, spin-coat it again, repeat the above operation 6 times, and sinter it at 400°C for 20 minutes in a reducing atmosphere (hydrogen to argon volume ratio of 1:4) to obtain porous titanium in direct contact with the FTO conductive glass;

[0113] The sheet resistance of the porous titanium FTO conductive glass prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 2.

[0114] The porous titanium FTO conductive glass prepared above was placed inside the ALD chamber after ultrasonic treatment with acetone, ethanol, and deionized water. The precursors were trimethylaluminum (TMA, C3H9Al) and water (H2O), respectively. The reaction chamber pressure was 50Pa, and the carrier gas in the reaction chamber was nitrogen (flow rate was 20ml / min). The pulse time of TMA and water was 0.1s. First, the precursor trimethylaluminum was introduced into the reaction chamber in the form of pulses to react with the hydroxyl groups on the FTO conductive glass. The reaction product (-O-)Al(CH3)2 was adsorbed on the surface, and the gas reaction product CH4 and the excess precursor TMA were discharged from the reaction chamber by introducing the inert gas N2. After the first reaction is completed, the precursor water vapor is introduced to react with the reaction product just adsorbed. After the reaction reaches saturation, the reaction product and excess water vapor are discharged from the reaction chamber through nitrogen to obtain a single-layer Al2O3 film. At the same time, the surface of the aluminum oxide is covered with hydroxyl groups, and the next cycle reaction can be carried out. The thickness of the aluminum oxide film can be controlled by the number of cycles. The above operation is repeated 20 times to obtain an aluminum oxide film layer with a thickness of 2nm, and FTO conductive glass prepared with a porous Ti / aluminum oxide layer (mesoporous metal layer) is obtained;

[0115] A 10 μm thick layer of mesoporous carbon slurry was screen-printed on the porous Ti / alumina layer. After sintering at 400°C, the electrode layer and the mesoporous metal layer were filled with perovskite solution, and then heated and crystallized at 100°C for 0.5 h to obtain a mesoporous perovskite solar cell.

[0116] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Figure 5 As shown, the key electrical parameters are summarized in Example 2 in Table 2, wherein the FF is not higher than that of Comparative Example 1 due to the different structures (this example does not contain an insulating spacer layer).

[0117] Example 3

[0118] Provided is a mesoporous solar cell (inverted), which comprises, arranged from bottom to top in sequence, a conductive substrate (FTO conductive glass), a 100nm thick mesoporous metal layer (including porous nickel and a 3nm thick nickel oxide coating layer), a 2μm thick mesoporous insulating spacer layer (mesoporous aluminum oxide), and a 5μm thick electrode layer (mesoporous titanium), wherein the mesoporous metal layer, the mesoporous insulating spacer layer, and the electrode layer are all filled with perovskite.

[0119] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0120] The cleaned conductive substrate was treated with ultraviolet ozone (UVO) for 10 min, and then electrodeposited (the conductive substrate was used as the working electrode, Pt and Ag / AgCl were used as the counter electrode and reference electrode, respectively, and the deposition solution was a mixed solution of 1.0 mol / L NiSO4, 0.05 mol / L CuSO4 and 0.5 mol / L H3BO3). The cathode electrodeposition was carried out at a constant potential of -0.8 V, and the deposition charge was 0.5 C / cm 2 After cathode deposition, in the same three-electrode system, an anodic potential of 0.5 V was applied with a cutoff current density of 15.0 μA / cm to dissolve the metallic copper and obtain porous nickel in direct contact with the FTO conductive glass;

[0121] The sheet resistance of the porous nickel FTO conductive glass prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 3.

[0122] The FTO conductive glass prepared with porous nickel was placed inside the ALD chamber. Under the conditions of 40Pa pressure and 200℃ temperature, bis(dimethylamino-2-methyl-2-butoxy)nickel and water were used as nickel source and oxygen source respectively, and high-purity nitrogen was used as carrier gas. First, the nickel precursor was introduced into the chamber in pulse form to react with the conductive substrate. The pulse time was 4s. Then, the chamber was cleaned with nitrogen. The water vapor pulse duration was 6s. Nickel oxide was produced by reaction on the surface of the substrate. Nitrogen was introduced to purge the clean chamber to complete a cycle. The thickness of the nickel oxide film can be controlled by the number of cycles. The above operation was repeated 30 times to obtain a nickel oxide film layer with a thickness of 3nm, and the FTO conductive glass prepared with a porous nickel / nickel oxide layer (mesoporous metal layer) was obtained.

[0123] A 2 μm thick layer of mesoporous alumina slurry is screen-printed on the porous nickel / nickel oxide layer, and a 5 μm thick layer of mesoporous titanium slurry is printed after drying. After sintering at 300°C, the electrode layer, mesoporous insulating spacer layer and mesoporous metal layer are filled with perovskite solution, and dried at 100°C for 10 minutes to obtain a mesoporous perovskite solar cell.

[0124] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Figure 6 As shown, the key electrical parameters are summarized in Table 2 for Example 3.

[0125] Example 4

[0126] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a 300nm thick mesoporous metal layer (including porous aluminum and a 0.5nm thick magnesium oxide coating layer), and a 10μm thick electrode layer (mesoporous carbon) arranged in sequence from bottom to top, wherein the mesoporous metal layer and the electrode layer are both filled with perovskite.

[0127] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0128] Mix nano-aluminum particles (particle size of 50-100 nm) with acetone, iodine, low-concentration hydrochloric acid and deionized water (in the mixed solution, 0.06 g / ml of aluminum nano-particles, 0.05 g / ml of acetone, 0.05 g / ml of iodine, pH value of 2), and treat with ultrasonic vibration in a low-temperature ice bath to form a stable colloid. After sedimentation, take the upper clear colloid solution for use;

[0129] Two FTO electrodes are used as working electrodes and counter electrodes respectively, and the bias voltage is set to 5V. The polarized nanoparticles reach the anode FTO surface under the action of the electric field and adhere to the electrode surface. The thickness of the aluminum particle attachment layer is linearly positively correlated with the bias treatment time. Different thicknesses of aluminum particle layers can be obtained by setting different times. In this embodiment, a porous aluminum layer with a thickness of 300nm is obtained by depositing for 70s. It is sintered at 400℃ for 20min in a reducing atmosphere (hydrogen and nitrogen volume ratio is 1:4) to obtain porous aluminum in direct contact with the FTO conductive glass.

[0130] The sheet resistance of the FTO conductive glass with porous aluminum prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 4.

[0131] The FTO conductive glass prepared with porous aluminum was placed in a nitrogen environment, and a 1 mM concentration of magnesium acetate aqueous solution was spin-coated on the surface of the FTO conductive glass prepared with porous aluminum, and then dried and treated at 350° C. for 10 min to obtain the FTO conductive glass prepared with a porous aluminum / magnesium oxide layer (mesoporous metal layer);

[0132] A 20 μm thick layer of mesoporous carbon slurry was screen-printed on the porous aluminum / magnesium oxide layer. After sintering at 400°C, the perovskite solution was filled into the electrode layer and the mesoporous metal layer, and crystallized at 57°C for 20 hours to obtain a mesoporous perovskite solar cell.

[0133] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Figure 7 As shown, the key electrical parameters are summarized in Example 4 in Table 2, wherein the performance is not as high as that of Comparative Example 1, which is due to the different structure (this example does not contain a mesoporous insulating spacer layer).

[0134] Example 5

[0135] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a 200nm thick mesoporous metal layer (including a porous copper and titanium oxide coating layer), a 2μm thick mesoporous insulating spacer layer (mesoporous aluminum oxide) and a 15μm thick electrode layer (mesoporous nickel) which are arranged in sequence from bottom to top.

[0136] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0137] The copper and magnesium targets and substrates were installed on the magnetron sputtering equipment, and the coating vacuum was 5Pa. By keeping the turntable speed at 10rpm, controlling the sputtering parameters of Ar flow rate 20sccm, power 50W, and sputtering time 25 min, an alloy film was obtained, in which the composition ratio of copper to magnesium alloy was 30:70 and the thickness was 400nm. Under room temperature conditions, the prepared alloy film was immersed in 1.00mol / L HCl solution to remove magnesium. When no bubbles were generated on the surface of the sample, it was repeatedly washed with deionized water, and then placed in a drying oven for vacuum drying to avoid oxidation of the sample, and porous copper in direct contact with the FTO conductive glass was obtained;

[0138] The sheet resistance of the FTO conductive glass with porous copper prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 5.

[0139] The FTO conductive glass prepared with porous copper was placed in a vacuum chamber, immersed in a 40 mM titanium tetrachloride aqueous solution at 70°C for 30 minutes, a layer of titanium oxide was formed on the surface, and then sintered at 400°C to obtain the FTO conductive glass prepared with a porous copper / titanium oxide layer;

[0140] A 2 μm thick layer of mesoporous alumina slurry is screen-printed on the porous copper / titanium oxide layer, and a 15 μm thick layer of mesoporous nickel slurry is printed after drying. After sintering at 300°C, the electrode layer, mesoporous insulating spacer layer and mesoporous metal layer are filled with perovskite solution, and crystallized at 57°C for 20 hours to obtain a mesoporous perovskite solar cell.

[0141] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Figure 8 As shown, the key electrical parameters are summarized in Table 2 for Example 5.

[0142] Example 6

[0143] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a 350nm thick mesoporous metal layer (including porous titanium and a 2nm aluminum oxide coating layer), and a 10μm thick electrode layer (mesoporous carbon) which are arranged in sequence from bottom to top, wherein the mesoporous metal layer and the electrode layer are both filled with perovskite.

[0144] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0145] Nano-titanium, citric acid, stabilizer (tetraoctylammonium bromide), and isopropanol were mixed in a mass ratio of 1:0.3:0.01:100, stirred and ultrasonically dispersed at -5°C to obtain a nano-titanium dispersion with a concentration of 0.01 mg / ml;

[0146] Spin-coat the nano-titanium dispersion on the FTO conductive glass at a speed of 3000 rpm / min to a thickness of about 40 nm, dry it, spin-coat it again, repeat the above operation 9 times, and sinter it at 400°C for 20 minutes in a reducing atmosphere (hydrogen to argon volume ratio of 1:4) to obtain porous titanium in direct contact with the FTO conductive glass;

[0147] The sheet resistance of the porous titanium FTO conductive glass prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 6.

[0148] The FTO conductive glass prepared with porous titanium was immersed in a colloid solution of magnesium oxide (the preparation method of the colloid solution of magnesium oxide is as follows: 28 mg of iodine and 4 ml of acetone were mixed in 250 ml of anhydrous ethanol, 0.3 g of magnesium ethoxide was added, stirred and added to the ethanol in an ice water bath, ultrasonically dispersed until the magnesium ethoxide was dissolved, 2 ml of deionized water and 5 ml of nitric acid were added, and stirred for 24 h, centrifuged at 400 rpm, and the precipitate was removed to obtain a colloid solution of magnesium oxide). The constant current method was used, and the current density was 0.01 mA / cm 2 During the deposition process, magnesium oxide causes electrode passivation, increases resistance, and increases the voltage of the system. The cut-off voltage is 1V, and the deposition is stopped to obtain FTO conductive glass prepared with a porous titanium / magnesium oxide layer (mesoporous metal layer);

[0149] The perovskite precursor solution is spin-coated on the deposited titanium and magnesium oxide electrodes, dried at 100°C, and then a 10-micron thick layer of low-temperature carbon is printed and dried to complete the battery preparation and testing.

[0150] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Fig. 9 As shown, the key electrical parameters are summarized in Table 2 Example 6, by Fig. 9It can be seen that the FF reaches 79% and the series resistance is 24 ohms. The structure of this embodiment is different from that of comparative example 1. There is only one mesoporous layer, the middle is a perovskite layer, and the electrode layer is carbon.

[0151] Example 7

[0152] Provided is a mesoporous solar cell, which comprises a conductive substrate (FTO conductive glass) and a mesoporous metal layer with a thickness of 3 μm (including porous titanium and a titanium oxide coating layer with a thickness of 2 nm) which are arranged in sequence from bottom to top, wherein the mesoporous metal layer is adsorbed with N719 dye.

[0153] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0154] Nano-titanium was mixed with ethyl cellulose, pinene alcohol, ethanol and citric acid in a mass ratio of 1:1:7:50:0.01, and ball-milled at a speed of 300 rpm for 20 h. After ball-milling, the mixture was rotary evaporated at 40°C and 0.01 MPa for 20 h to obtain nano-Ti slurry.

[0155] A layer of nano-Ti slurry was printed on the FTO conductive glass and sintered at 400°C for 20 min in a reducing atmosphere (hydrogen to nitrogen volume ratio of 1:4) to obtain porous titanium in direct contact with the FTO conductive glass.

[0156] The sheet resistance of the porous titanium FTO conductive glass prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 7.

[0157] The FTO conductive glass prepared with porous titanium was placed in a vacuum chamber, immersed in a 40 mM titanium tetrachloride aqueous solution at 70°C for 30 minutes, a layer of titanium oxide was formed on the surface, and then sintered at 400°C to obtain FTO conductive glass prepared with a porous Ti / titanium oxide layer (mesoporous metal layer);

[0158] The FTO conductive glass prepared with porous Ti / titanium oxide layer was immersed in N719 dye for 20 hours, at which time, the N719 dye was adsorbed on the titanium oxide surface. The counter electrode was an FTO electrode (with a through hole diameter of 0.1 mm) printed with PT1 platinum paste (greatcellsolar). The PT1 platinum paste was printed and sintered at 400℃ for 20 minutes to obtain a platinum electrode with a thickness of 100nm. The electrolyte was a commercial iodine-containing electrolyte EL-HSE High Stability Electrolyte (greatcellsolar). The electrolyte was encapsulated with a sarin membrane. Specifically, the two electrodes were separated face to face with sarin membrane, heated to 100℃ and kept for 10 minutes, and the two electrodes were encapsulated together. The electrolyte was injected through the back electrode through hole and the through hole was encapsulated with a sarin membrane to obtain a mesoporous dye-sensitized solar cell.

[0159] The obtained mesoporous dye-sensitized solar cell was subjected to IV test, and the test results are as follows: Fig.10 As shown, the key electrical parameters are summarized in Table 2 for Example 7.

[0160] Example 8

[0161] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a 300nm thick mesoporous metal layer (including porous aluminum and a 2nm aluminum nitride coating layer), and a 10μm thick electrode layer (mesoporous carbon) which are arranged in sequence from bottom to top, wherein the mesoporous metal layer and the electrode layer are both filled with perovskite.

[0162] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0163] Nano-aluminum, citric acid, stabilizer (tetraoctylammonium bromide), and isopropanol were mixed in a mass ratio of 1:0.3:0.01:200, stirred and ultrasonically dispersed at -5°C to obtain a nano-aluminum dispersion with a concentration of 0.005 mg / ml;

[0164] Spin-coat the nano-aluminum dispersion on the FTO conductive glass at a speed of 3000 rpm / min to a thickness of about 40 nm, dry it, spin-coat it again, repeat the above operation 5 times, and sinter it at 300°C for 20 minutes in a reducing atmosphere (hydrogen to argon volume ratio of 1:4) to obtain porous aluminum in direct contact with the FTO conductive glass;

[0165] The sheet resistance of the FTO conductive glass with porous aluminum prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 8.

[0166] The FTO conductive glass prepared with porous aluminum is placed inside the ALD chamber, and the substrate temperature is set to 350°C. The precursors are trimethylaluminum (TMA, C3H9Al) and ammonia (NH3), the reaction chamber pressure is 50 mBar, the carrier gas in the reaction chamber is nitrogen (flow rate is 20ml / min), and the pulse times of TMA and ammonia are 0.1 and 5s, respectively. First, the precursor trimethylaluminum is introduced into the reaction chamber in the form of a pulse and adsorbed on the substrate. After purging, the precursor ammonia is introduced and reacts with the just adsorbed TMA at high temperature. The reaction products and excess ammonia are discharged from the reaction chamber through nitrogen to obtain a single-layer AlN film. The thickness of the aluminum nitride film can be controlled by the number of cycles. The above operation is repeated 10 times to obtain an aluminum nitride film layer with a thickness of 1nm, and the FTO conductive glass prepared with a porous aluminum / aluminum nitride layer (mesoporous metal layer) is obtained;

[0167] The perovskite precursor solution is spin-coated on the deposited aluminum and aluminum nitride electrodes, dried at 100°C, and then a 10-micron thick layer of low-temperature carbon is printed and dried to complete the battery preparation and testing.

[0168] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Fig. 9 As shown, the key electrical parameters are summarized in Example 8 in Table 2. The structure of this example is different from that of Comparative Example 1. It has only one mesoporous layer, a perovskite layer in the middle, and a carbon electrode layer.

[0169] Example 9

[0170] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass) arranged in sequence from bottom to top, a mesoporous copper with a thickness of 150 nm, a single molecule layer adsorbed on the copper surface, generally a self-assembled monolayer (SAM) containing a thiol group is selected, which can be anchored on the metal surface, and the end can be a long-chain alkyl or benzene ring group or other functional group, and its length determines the thickness of a covering layer formed on the metal surface, and finally a 10 μm thick electrode layer (mesoporous carbon), wherein the mesoporous metal layer and the electrode layer are both filled with perovskite.

[0171] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0172] Nano copper, citric acid, stabilizer (tetraoctylammonium bromide), and isopropanol were mixed in a mass ratio of 1:0.3:0.01:100, stirred and ultrasonically dispersed at -5°C to obtain a nano copper dispersion with a concentration of 0.01 mg / ml;

[0173] Spin-coat the nano-copper dispersion on the FTO conductive glass, and spin-coat the nano-aluminum dispersion at a speed of 3000 rpm / min to a thickness of about 30 nm. After drying, spin-coat again. Repeat the above operation 5 times, and sinter at 350°C for 20 minutes in a reducing atmosphere (hydrogen to argon volume ratio of 1:4) to obtain porous copper in direct contact with the FTO conductive glass.

[0174] The sheet resistance of the FTO conductive glass with porous copper prepared in this embodiment was tested using an FT-331 ordinary four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Example 9.

[0175] The FTO conductive glass prepared with porous copper is immersed in an ethanol solution of octanethiol for 8 hours, the concentration of which is 3 mM, and then washed with ethanol to obtain an FTO conductive glass prepared with a porous copper layer (mesoporous metal layer) modified with octanethiol;

[0176] The perovskite precursor solution was spin-coated on the copper electrode adsorbed with octanethiol, dried at 100°C, and then a layer of 10-micron-thick low-temperature carbon was printed and dried to complete the battery preparation and testing.

[0177] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Fig. 9 As shown, the key electrical parameters are summarized in Example 9 in Table 2. The structure of this example is different from that of Comparative Example 1. It has only one mesoporous layer, a perovskite layer in the middle, and a carbon electrode layer.

[0178] Comparative Example 1

[0179] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a mesoporous titanium oxide layer with a thickness of 150 nm, a mesoporous insulating spacer layer (mesoporous zirconium oxide) with a thickness of 1 μm, and an electrode layer (mesoporous carbon) with a thickness of 10 μm, which are arranged in sequence from bottom to top, wherein the mesoporous metal layer, the mesoporous insulating spacer layer and the electrode layer are all filled with perovskite.

[0180] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0181] 150nm mesoporous titanium oxide slurry was printed on FTO conductive glass and annealed at 500℃ for 30min;

[0182] A 1 μm thick layer of mesoporous zirconia slurry is screen-printed on the mesoporous titanium oxide, and a 10 μm thick layer of mesoporous carbon slurry is printed after drying. After sintering at 400°C, the electrode layer, the mesoporous insulating spacer layer and the mesoporous metal layer are filled with perovskite solution, and crystallized at 57°C for 20 hours to obtain a mesoporous perovskite solar cell.

[0183] The sheet resistance of the FTO conductive glass in this embodiment was tested using an FT-331 common four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test data is shown in Table 1 Comparative Example 1.

[0184] The obtained mesoporous perovskite solar cell was subjected to IV test, and the test results are as follows Fig.11 As shown, the key electrical parameters are summarized in Table 2 for Comparative Example 1.

[0185] Comparative Example 2

[0186] Provided is a mesoporous solar cell, comprising a conductive substrate (FTO conductive glass) and a mesoporous titanium oxide layer with a thickness of 3 μm, which are arranged in sequence from bottom to top, wherein the mesoporous titanium oxide layer is adsorbed with N719 dye.

[0187] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0188] A 3 μm mesoporous titanium oxide slurry was printed on the FTO conductive glass, and sintered at 500° C. for 30 min to obtain the FTO conductive glass prepared with a mesoporous titanium oxide layer;

[0189] The FTO conductive glass prepared with a mesoporous titanium oxide layer was immersed in N719 dye for 20 hours. At this time, the N719 dye was adsorbed on the titanium oxide surface. The counter electrode was an FTO electrode (with a through-hole diameter of 0.1 mm) printed with PT1 platinum paste (greatcellsolar). The PT1 platinum paste was printed and sintered at 400°C for 20 minutes to obtain a platinum electrode with a thickness of ~100 nm. The electrolyte was a commercial iodine-containing electrolyte EL-HSE High Stability Electrolyte (greatcellsolar). The electrolyte was encapsulated with a sarin membrane. Specifically, the two electrodes were separated face to face with a sarin membrane, heated to 100°C and maintained for 10 minutes, and the two electrodes were encapsulated together. The electrolyte was injected through the back electrode through-hole and the through-hole was encapsulated with a sarin membrane to obtain a mesoporous dye-sensitized solar cell. The obtained mesoporous dye-sensitized solar cell was subjected to IV testing, and the test results are shown as follows. Fig.10 As shown, the key electrical parameters are summarized in Table 2 for Comparative Example 2.

[0190] Depend on Fig.10 It can be seen that compared with Comparative Example 2, the internal resistance of the mesoporous dye-sensitized solar cell obtained in Example 7 is slightly lower, thanks to the low resistivity of the metal. However, since the thicker film layer affects the transmittance of light (not within the optimal range), its electrical properties such as current are poor. Example 7 only confirms the feasibility of photosensitizing dyes and does not focus on optimizing their performance.

[0191] Comparative Example 3

[0192] Provided is a mesoporous solar cell, which includes a conductive substrate (FTO conductive glass), a mesoporous metal layer (including porous titanium) with a thickness of 150 nm, a mesoporous insulating spacer layer (mesoporous zirconia) with a thickness of 1 μm, and an electrode layer (mesoporous carbon) with a thickness of 10 μm, which are arranged in sequence from bottom to top, wherein the mesoporous metal layer, the mesoporous insulating spacer layer and the electrode layer are all filled with perovskite.

[0193] The preparation method of the above-mentioned mesoporous solar cell is as follows:

[0194] Nano-titanium was mixed with ethyl cellulose, pinene alcohol, ethanol and citric acid in a mass ratio of 1:1:7:50:0.01, and ball-milled at a speed of 300 rpm for 20 h. After ball-milling, the mixture was rotary evaporated at 40°C and 0.01 MPa for 20 h to obtain nano-Ti slurry.

[0195] A layer of nano-Ti slurry was printed on the FTO conductive glass and sintered at 400°C for 20 min in a reducing atmosphere (hydrogen to nitrogen volume ratio of 1:4) to obtain a porous titanium layer in direct contact with the FTO conductive glass.

[0196] A 1 μm thick layer of mesoporous zirconia slurry is screen-printed on the porous titanium layer, and a 10 μm thick layer of mesoporous carbon slurry is printed after drying. After sintering at 400°C, perovskite is filled into the electrode layer, mesoporous insulating spacer layer and mesoporous metal layer, and crystallized at 57°C for 20 hours to obtain a mesoporous perovskite solar cell.

[0197] The obtained mesoporous solar cell was subjected to IV test, and the test results are as follows Fig.12 As shown, since the mesoporous metal in the mesoporous metal layer is not surface treated to form a modified layer, the perovskite directly contacts the FTO and the mesoporous metal, resulting in serious composite and poor performance. The key electrical parameters are summarized in Table 2 for Comparative Example 3.

[0198] Performance Testing

[0199] (1) The sheet resistance of the conductive substrates prepared with porous metal in Examples 1 to 9 and Comparative Example 1 was tested using an FT-331 common four-probe sheet resistance resistivity tester in a nitrogen-filled glove box. The test results are shown in Table 1.

[0200] Table 1 Sheet resistance of the conductive substrate prepared with porous metal in Examples 1 to 9 and Comparative Example 1

[0201]

[0202] It can be seen from Table 1 that the square resistance of the conductive substrates prepared with porous metal in Examples 1 to 9 is less than 2, while the square resistance of the FTO conductive glass in Comparative Example 1 is as high as 15 Ω / □. This indicates that the use of porous metal in contact with FTO conductive glass can reduce the square resistance of the FTO conductive glass electrode.

[0203] (2) The mesoporous solar cells obtained in Examples 1 to 9 and Comparative Examples 1 to 3 were subjected to IV tests. The key electrical parameters are shown in Table 2.

[0204] Table 2 Key electrical parameters of mesoporous solar cells obtained in Examples 1 to 9 and Comparative Examples 1 to 3

[0205]

[0206] It can be seen from Table 2 that:

[0207] Compared with Examples 1 to 6 and Examples 8 and 9, the internal resistance Rs of the battery in Comparative Example 1 using mesoporous oxide instead of the porous metal layer is as high as 43, while the internal resistance Rs of the battery obtained in Examples 1 to 6 and Examples 8 and 9 are all lower than 40. Therefore, the use of porous metal can reduce the internal resistance of the battery.

[0208] Compared with Examples 1 to 6 and Examples 8 and 9, the mesoporous perovskite solar cell without a modified layer in Comparative Example 3 has a low photoelectric conversion efficiency (FF), indicating that carriers recombine severely at the porous metal interface.

[0209] Both Example 1 and Comparative Example 1 are batteries with three-layer mesoporous structures. The electrical performance of the battery obtained in Example 1 is better than that in Comparative Example 1, which shows that the mesoporous solar cell provided by the present invention has the technical effects of low internal resistance and high photoelectric conversion efficiency.

[0210] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A mesoporous solar cell, characterized in that: It comprises a conductive substrate, and a mesoporous metal layer and an electrode layer sequentially arranged on the conductive substrate; Wherein, the mesoporous metal layer comprises a porous metal and a modified layer attached to the surface of the porous metal; the conductive substrate is in contact with the porous metal; The modified layer includes at least one of metal oxide, metal nitride and epoxy resin; At least the pores of the porous metal are filled with photosensitizing material.

2. The mesoporous solar cell according to claim 1, characterized in that: The material of the porous metal includes at least one of titanium, nickel, aluminum, manganese, tin, niobium, tantalum, copper, cobalt, indium, and tungsten.

3. The mesoporous solar cell according to claim 1, characterized in that: The metal oxide includes at least one of titanium dioxide, aluminum oxide, nickel dioxide and magnesium oxide; and / or, The metal nitride includes at least one of aluminum nitride, gallium nitride and indium nitride.

4. The mesoporous solar cell according to claim 1, characterized in that: The thickness of the mesoporous metal layer is 100 nm to 1000 nm; and / or, The pore size of the porous metal is 10nm~1000nm; and / or, The thickness of the modified layer is 0.1 nm to 4 nm.

5. The mesoporous solar cell according to claim 1, characterized in that: A mesoporous insulating spacer layer is also arranged between the mesoporous metal layer and the electrode layer.

6. The mesoporous solar cell according to claim 1, characterized in that: The photosensitizing material includes at least one of a perovskite material and a photosensitizing dye.

7. A method for preparing a mesoporous solar cell according to any one of claims 1 to 6, characterized in that: The following steps are involved: preparing porous metal on a conductive substrate; preparing a modified layer on the surface of the porous metal to obtain a mesoporous metal layer; At least an electrode layer is prepared on the surface of the mesoporous metal layer to obtain a mesoporous solar cell; Wherein, at least the pores of the mesoporous metal layer are filled with photosensitizing material.

8. The method for preparing a mesoporous solar cell according to claim 7, characterized in that: The step of preparing porous metal on a conductive substrate comprises: The nano-metal is mixed with ethyl cellulose, pine alcohol, ethanol and citric acid, ball-milled, and distilled under reduced pressure to obtain a metal slurry; The metal slurry is deposited on a conductive substrate and sintered in a reducing atmosphere to prepare a porous metal.

9. The method for preparing a mesoporous solar cell according to claim 8, characterized in that: In the step of depositing the metal slurry on the conductive substrate and sintering in a reducing atmosphere to prepare the porous metal, the sintering temperature is 300-550°C.

10. The method for preparing a mesoporous solar cell according to claim 8, characterized in that: In the step of mixing the nano metal with ethyl cellulose, pinene alcohol, ethanol and citric acid, ball milling, and performing reduced pressure distillation to obtain the metal slurry: The mass ratio of the nano metal, ethyl cellulose, pinene alcohol, ethanol and citric acid is (1-2): 1: (7-10): (30-50): (0.001-0.01); and / or, The ball milling time is 8 to 20 hours; and / or, The temperature of the reduced pressure distillation is 40-50°C; and / or, The pressure of the reduced pressure distillation is 0.01-0.02 MPa; and / or, The particle size of the nano metal is 20-200 nm.