High-color-purity multicolor electroluminescent fiber as well as preparation method and application thereof

Through the grafting modification of lead halide perovskite quantum dot nanomaterials, the problem of single color and low purity of electroluminescent fibers has been solved, the preparation of multi-color fibers with high color purity has been achieved, the color gamut has been broadened, and it is suitable for flexible applications. Display and smart clothing fields.

CN118870931AActive Publication Date: 2024-10-29FUDAN UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410854232.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing electroluminescent fibers face the problems of single display color and poor color purity, and cannot meet flexible and diverse display needs.

Method used

Lead halide perovskite quantum dot nanomaterials are used for grafting and modification, and by regulating the type and proportion of halogens, high-color purity multi-color electroluminescent fibers are prepared to broaden the color gamut.

Benefits of technology

The electroluminescent fiber that achieves high color purity and wide color gamut is suitable for diversified luminescent color displays. The process is simple and the conditions are mild, making it suitable for applications such as weaving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118870931A_ABST
    Figure CN118870931A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of intelligent electronic devices, and particularly relates to a high-color-purity multicolor electroluminescent fiber and a preparation method and application thereof. The preparation method of the fiber comprises the following steps: preparing lead halide perovskite type nano quantum dots as light conversion particles through a thermal injection method, a room-temperature supersaturated recrystallization method and the like; the lead halide perovskite type nano quantum dots are grafted and modified on the surfaces of metal sulfide type electroluminescent particles through surface ligands to obtain the high-color-purity multicolor electroluminescent active material. Compounding the light conversion particle modified electroluminescent active material and a transparent thermoplastic elastomer polymer to obtain active slurry, and coating the active slurry on the surface of the conductive fiber through a continuous confinement coating process; and loading an outer electrode on the coated conductive fiber to obtain the high-color-purity multicolor electroluminescent fiber. The multicolor electroluminescent fiber prepared by the invention has various colors and high color purity, and meets the color gamut range required by luminescent fiber and display fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of intelligent electronic devices, and in particular relates to a high-color-purity multi-color electroluminescent fiber and a preparation method and application thereof. Background Art

[0002] In recent years, with the cross-integration of materials science, information technology and medicine, people have put forward more and more demands on electronic devices, such as flexibility, wearability, self-healing and other characteristics. Vision is the main source of human beings to obtain external information, and traditional display devices have been difficult to meet the development requirements of flexible display devices for flexibility, lightness and portability. Considering that they need to face various complex deformations such as twisting, bending, stretching, etc. during the application process, fabric luminous display devices show unique advantages. They can be obtained by weaving electroluminescent fibers, and pattern display, information interaction and other functions can be realized through circuit design. Therefore, as a new type of flexible intelligent electronic device, it has received widespread attention from the scientific and industrial communities. Among them, the performance of luminous fibers is the key factor that determines the performance of display fabrics, including pixel density, color type, brightness and purity.

[0003] However, electroluminescent fibers currently face the challenge of displaying a single color and poor color purity. In patent CN202310048457.9, a new luminescent color is compounded by adding micron-sized fluorescent pigment particles to the luminescent slurry, but the phosphor, as a down-conversion material, has a wide spectrum and the fiber luminescent color is not pure enough. Another document "Color-tunable light-emitting fibers for pattern displaying textiles" J. Mater. Chem. C, 2024, 12, 941 reports that a double luminescent layer is constructed with zinc sulfide luminescent powders that emit orange and blue light to achieve dynamic color adjustment, but the emitted spectrum is actually a composite color of two lights, resulting in low brightness, a very limited color range, and poor color purity.

[0004] Quantum dot materials are a type of semiconductor nanocrystals with excellent optoelectronic properties. They can absorb light from the ultraviolet to visible light bands and perform down-conversion to emit visible light of other colors. These lights have very narrow half-peak widths and very high color purity, which is higher than the color standards of LCD TVs and the National Television Standards Committee of the United States. Using quantum dot materials in the preparation of light-emitting fiber devices can obtain more positive luminescent colors.

[0005] To this end, the present invention proposes a strategy of using lead halide perovskite quantum dot nanomaterials as light conversion materials and grafting and modifying traditional electroluminescent materials to prepare a new type of electroluminescent material, thereby obtaining a high color purity multi-color electroluminescent fiber. By adjusting the type and proportion of halogen, the color gamut of the electroluminescent fiber is broadened. Summary of the invention

[0006] The purpose of the present invention is to provide a high-color-purity multi-color electroluminescent fiber and its preparation method and application, based on the problem that electroluminescent fibers display a single color and poor color purity, so as to achieve diversification of luminous colors and improve color purity and color gamut range.

[0007] The high color purity multi-color electroluminescent fiber provided by the present invention is obtained by grafting lead halide perovskite quantum dot nanomaterials onto the surface of traditional AC electroluminescent particles, and directionally controlling the luminescent color by changing the composition and proportion of the quantum dot materials, thereby obtaining a high color purity multi-color electroluminescent fiber.

[0008] The specific steps of the preparation method are as follows:

[0009] (1) Preparation of quantum dot photoconversion particles: Preparation of lead halide perovskite nano-quantum dots (CsPbX3 QDs) as photoconversion particles by hot injection method, room temperature supersaturated recrystallization method, etc.;

[0010] (2) Preparation of electroluminescent active materials modified with light-converting particles: Lead halide perovskite nano-quantum dots are grafted onto the surface of metal sulfide electroluminescent particles through surface ligands to obtain high color purity multi-color electroluminescent active materials; the color of the electroluminescent active materials can be directionally controlled by changing the type and ratio of halogen in the perovskite nano-quantum dot material;

[0011] (3) Loading the luminescent active layer: Compounding the electroluminescent active material modified by the light conversion particles and the transparent thermoplastic elastomer polymer to obtain a uniform and stable luminescent active slurry, and coating the luminescent active slurry on the surface of the conductive fiber through a continuous confined coating process to obtain a conductive fiber coated with the electroluminescent active layer;

[0012] (4) Loading fiber external electrode: The external electrode is loaded on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain high color purity multi-color electroluminescent fiber, and the luminescent colors are pure red, orange, yellow, green, blue, purple, and white.

[0013] In the present invention, in step (1), the types of halogen in the perovskite nano-quantum dots are Cl, Br, and I, and the size of the perovskite nano-quantum dots is 5-20 nm.

[0014] In the present invention, in step (1), the specific steps of the hot injection method are:

[0015] 0.276-0.4 g Cs2CO3, 10-15 mL octadecene (ODE) and 0.833-1.76 mL surface ligand are selected, mixed and stirred, and placed in a three-necked flask, heated to 120-140° C. under N2 atmosphere and dried for 0.5-1 hour to obtain a cesium oleate precursor solution;

[0016] 0.376-0.752mmol PbX2 (X = Cl, Br, I) and 10-20mL ODE are placed in a 100mL flask, heated to 120-140°C under N2 atmosphere and dried for 0.5-1 hour; then, 1-2mL of surface ligand is slowly injected into the flask under stirring, and stirred until the solution becomes clear; the flask is heated to 160-180°C, and 0.8-1.6mL of cesium oleate precursor solution is quickly injected, and after standing for 5-10s, the mixture solution is cooled to room temperature using an ice water bath; it is washed with an antisolvent and redispersed in 1-2mL of toluene or n-hexane for further use.

[0017] Furthermore, the surface ligand is a mixture of one or more of oleic acid (OA), oleylamine (OAm), 3-aminopropyltriethoxysilane (APTES), and trioctylphosphine (TOP).

[0018] Furthermore, the anti-solvent is ethyl acetate or methyl acetate.

[0019] In the present invention, in step (1), the room temperature supersaturated recrystallization method specifically comprises the following steps:

[0020] Dissolve 0.4-0.8mmol PbX2 and 0.4-0.8mmol CsX (X=Cl, Br, I) in 10mL DMF or DMSO, add 1mL surface ligand to stabilize the precursor solution; then, under vigorous stirring, quickly add 0.5-1mL precursor solution into 10mL toluene.

[0021] Furthermore, the surface ligand includes a mixture of one or more of oleic acid (OA), oleylamine (OAm), and 3-aminopropyltriethoxysilane (APTES).

[0022] In the present invention, in step (2), the grafting modification method includes two methods, specifically:

[0023] Method 1: 0.5-1g of electroluminescent particles are mixed with 2mL of perovskite nanocrystal solution, 2-5μL of deionized water is added, and the mixture is stirred at 60-80°C for 24-30 hours; then, 5-20μL of silane coupling agent and 2-5μL of deionized water are added, and the mixture is stirred at 60-80°C for 6-8 hours; the precipitate is collected by centrifugation, and washed three times with toluene; and dried under vacuum to obtain an electroluminescent active material modified with nano-quantum dots;

[0024] or:

[0025] Method 2: Add 5 μL of silane coupling agent to 2 mL of perovskite nanocrystal solution, sonicate and stir for 1 hour; add 0.5-1.2 g of electroluminescent particles, 5-10 μL of silane coupling agent and 2-5 μL of deionized water, stir at 45°C for 24-32 hours; collect the precipitate by centrifugation, wash it with toluene three times; dry it under vacuum to obtain the electroluminescent active material modified with nano-quantum dots;

[0026] When the hot injection method is used in step (1), the grafting modification method in step (2) is method 1 or method 2;

[0027] When the room temperature supersaturated recrystallization method is used in step (1), the grafting modification method in step (2) is method 2.

[0028] Furthermore, the electroluminescent particles are CaS, SrS or ZnS.

[0029] Furthermore, the silane coupling agent is 3-aminopropyltriethoxysilane (APTES), γ-mercaptopropyltriethoxysilane (MPTES) or γ-mercaptopropyltrimethoxysilane (MPTMS).

[0030] In the present invention, in step (2), the particle size of the electroluminescent active material modified by nano-quantum dots obtained is 0.5-5 μm; the thickness of the electroluminescent active layer is 10-50 μm.

[0031] In the present invention, in step (3), the conductive fiber is a metal conductive fiber, an ion gel fiber or a conductive polymer composite fiber.

[0032] In the present invention, in step (3), the transparent thermoplastic elastomer polymer is polyester polyurethane, fluororubber or thermoplastic polyolefin elastomer.

[0033] In the present invention, in step (3), the diameter of the conductive fiber is 50-120 μm; the resistance of the conductive fiber is 5-50 Ω / m.

[0034] In the present invention, in step (3), the coating thickness of the electroluminescent active layer is 10-50 μm.

[0035] In the present invention, in step (3), the coating process is a conventional process, specifically: dipping and heating curing, the dipping speed is 0.1-1m / min, and the heating temperature is 60-100°C.

[0036] In the present invention, in step (4), the external electrode is a metal wire, such as a copper wire, a silver wire, a stainless steel wire or an aluminum wire; the diameter of the metal wire is 30-80 μm, and the resistance is 0.5-50 Ω / m.

[0037] In the present invention, in step (4), the twisting or twisting process is specifically: the pitch is 0.1-2mm, and the speed is 1-10m / min.

[0038] In the present invention, the high color purity multi-color electroluminescent fiber obtained by the above preparation method comprises, from the inside to the outside, a conductive fiber, a luminescent active layer, and an external electrode, forming an electrode-luminescent layer-electrode, i.e., a "sandwich" structure.

[0039] The diameter of the luminous fiber is 0.20-0.25 mm, the luminous brightness is 30-60 cd / m2, and the luminous colors include pure red, orange, yellow, green, blue, purple, and white, with high color purity.

[0040] In the present invention, the high color purity multi-color electroluminescent fiber can be used as clothing material in the production of clothing by weaving, embroidery and knitting.

[0041] Compared with the prior art, the present invention has the following advantages:

[0042] (1) The traditional luminescent materials are modified by grafting lead halide perovskite quantum dots to synthesize new luminescent-light-conversion electroluminescent materials. The emission spectrum obtained by changing the size of quantum dots and the halogen composition has high color purity and wide color gamut;

[0043] (2) The process of the present invention is simple and the conditions are mild. The prepared luminescent fibers have various colors and good flexibility. They can be woven, embroidered, knitted, etc., and have important application value in the field of smart clothing. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 Schematic diagram of the structure of high color purity multi-color electroluminescent fiber.

[0045] Figure 2 The electroluminescent spectra of blue, green and red light-emitting fibers are shown in Figure 4. In the figure, 4 is the spectrum curve of the blue light-emitting fiber, 5 is the spectrum curve of the green electroluminescent fiber, and 6 is the spectrum curve of the red electroluminescent fiber.

[0046] Figure 3The CIE color coordinate diagram of blue, green and red light-emitting fibers. In the figure, A is the CIE color coordinate of the blue light-emitting fiber, B is the CIE color coordinate of the green electroluminescent fiber, and C is the CIE color coordinate of the red electroluminescent fiber.

[0047] In the figure, the numbers 1 are conductive fibers, 2 are electroluminescent active layers, and 3 are external electrodes. Specific implementation methods

[0049] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0050] In the present invention, room temperature refers to an ambient temperature of 10-30°C.

[0051] The reagents used in the following examples are all purchased reagents, and various solvents are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. All equipment in the following examples are commercially available equipment.

[0052] Example 1

[0053] Step 1: Preparation of nano-quantum dots as photoconversion particles: 0.4g Cs2CO3, 15mL ODE and 1.76mL OA were placed in a 100mL three-necked flask under stirring, heated to 120°C under N2 atmosphere and dried for 1 hour. 0.376mmol PbBr2 and 10mL ODE were placed in a 100mL three-necked flask, heated to 120°C under N2 atmosphere and dried for 1 hour. Subsequently, 1mL OA and 1mL APTES were slowly injected into the second flask under stirring until the solution became clear. The temperature was raised to 160°C and 0.8mL Cs-OA precursor solution was quickly injected. After standing for 10 seconds, the mixture solution was cooled to room temperature using an ice-water bath to obtain CsPbBr3 quantum dots (particle size 10nm, green light). Wash and centrifuge with ethyl acetate at a speed of 11000rpm for 5min, and dispersed in 2mL n-hexane again.

[0054] Step 2: Preparation of a novel electroluminescent active material modified by nano-quantum dot grafting: 1 g of CaS was mixed with 2 mL of CsPbBr3 nano-quantum dot solution, 2 μL of deionized water was added, and the mixture was stirred at 80°C for 24 hours. Then, 10 μL of APTES and 2 μL of deionized water were added, and the mixture was stirred at 80°C for 6 hours. The precipitate was collected by centrifugation, washed three times with toluene, and dried under vacuum to obtain a novel electroluminescent active material CaS-g-CsPbBr3 QDs (particle size 0.5 μm, emitting green light) modified by nano-quantum dot grafting.

[0055] Step 3: Loading the luminescent active layer: Take 1g of polyurethane and 4g of the new electroluminescent active material, mix them evenly at room temperature to obtain a uniformly dispersed luminescent layer slurry. The active luminescent slurry is coated on the surface of a copper wire fiber with a diameter of 120μm through a 150μm limiting hole at a coating speed of 0.1m / min, and then heated and cured at 100℃ to obtain a conductive fiber loaded with a luminescent active layer.

[0056] Step 4: Loading external electrodes: Turn on the twisting device and load the copper fiber (30 μm in diameter) onto the fiber in step 3 at a twisting speed of 4 m / min and a pitch of 0.5 mm to obtain a green electroluminescent fiber with high color purity. The electroluminescent spectrum is shown in Figure 2 As shown by arrow 5, the CIE color coordinates are Figure 3 As shown in the middle circle B.

[0057] Example 2

[0058] Step 1: Preparation of nano-quantum dots as photoconversion particles: 0.276g Cs2CO3, 10mL ODE and 0.833mL OA were placed in a 100mL three-necked flask under stirring, heated to 140°C under N2 atmosphere and dried for 1 hour. 0.251mmol PbBr2, 0.501mmol PbI2 and 20mL ODE were placed in a 100mL three-necked flask, heated to 140°C under N2 atmosphere and dried for 1 hour. Subsequently, 2mL OA and 2mL OAm were slowly injected into the second flask under stirring until the solution became clear. The temperature was raised to 160°C and 2mL Cs-OA precursor solution was quickly injected. After standing for 5 seconds, the mixture solution was cooled to room temperature using an ice water bath to obtain CsPbBrI2 quantum dots (particle size 20nm, red light). Washed and centrifuged with methyl acetate at a speed of 11000rpm for 5min and dispersed in 2mL toluene again.

[0059] Step 2: Preparation of a novel electroluminescent active material modified by nano-quantum dot grafting: Add 5 μL MPTMS to 2 mL CsPbBrI2 nano-quantum dot solution, sonicate and stir for 1 hour. Add 0.5 g ZnS, 10 μL MPTMS and 5 μL deionized water, stir at 45 ° C for 32 hours. Collect the precipitate by centrifugation, wash three times with toluene, and dry under vacuum to obtain a novel electroluminescent active material ZnS-g-CsPbBrI2 (particle size 5 μm, red light) modified by nano-quantum dot grafting.

[0060] Step 3: Loading the luminescent active layer: Take 1g of polyurethane and 0.43g of the new electroluminescent active material, mix them evenly at room temperature to obtain a uniformly dispersed luminescent layer slurry. The active luminescent slurry is coated on the surface of a 50μm diameter silver-plated nylon fiber at a coating speed of 0.5m / min through a 120μm limiting hole, and then heated and cured at 80°C to obtain a conductive fiber loaded with a luminescent active layer.

[0061] Step 4: Loading external electrodes: Turn on the twisting device and load aluminum fibers (50 μm in diameter) onto the fibers in step 3 at a twisting speed of 1 m / min and a pitch of 0.1 mm to obtain a high-purity red electroluminescent fiber. The electroluminescent spectrum is shown in Figure 2 As shown by arrow 6, the CIE color coordinates are Figure 3 As shown in the middle circle C.

[0062] Example 3

[0063] Step 1: Preparation of nano-quantum dots as photoconversion particles: 0.4g Cs2CO3, 15mL ODE and 1.76mL OA were placed in a 100mL three-necked flask under stirring, heated to 120°C under N2 atmosphere and dried for 1 hour. 0.125mmolPbCl2, 0.251mmol PbBr2 and 10mL ODE were placed in a 100mL three-necked flask, heated to 120°C under N2 atmosphere and dried for 1 hour. Subsequently, 1mL TOP, 1mL OA and 1mL OAm were slowly injected into the second flask under stirring until the solution became clear. The temperature was raised to 180°C and 1mL Cs-OA precursor solution was quickly injected. After standing for 5 seconds, the mixture solution was cooled to room temperature using an ice water bath to obtain CsPbBr2Cl quantum dots (particle size 15nm, blue light). The mixture was washed with methyl acetate and centrifuged at 11000 rpm for 5 min, and then dispersed in 1 mL of n-octane.

[0064] Step 2: Preparation of a novel electroluminescent active material modified by nano-quantum dot grafting: Add 5 μL MPTES to 1 mL CsPbBr2Cl nano-quantum dot solution, sonicate and stir for 1 hour. Add 1 g SrS, 5 μL MPTES and 2 μL deionized water, stir at 45 ° C for 32 hours. Collect the precipitate by centrifugation and wash it three times with toluene. Dry under vacuum to obtain a novel electroluminescent active material SrS-g-CsPbBr2Cl (particle size 2 μm, blue light) modified by nano-quantum dot grafting.

[0065] Step 3: Loading the luminescent active layer: Take 1g of polyurethane and 3g of the new electroluminescent active material, mix them evenly at room temperature to obtain a uniformly dispersed luminescent layer slurry. The active luminescent slurry is coated on the surface of the conductive aramid fiber with a diameter of 80μm through a 180μm limiting hole at a coating speed of 1m / min, and then heated and cured at 60°C to obtain a conductive fiber loaded with a luminescent active layer.

[0066] Step 4: Loading external electrodes: Turn on the twisting device and load the stainless steel wire fiber (70 μm in diameter) onto the fiber in step 3 at a twisting speed of 10 m / min and a pitch of 2 mm to obtain a high-color-purity blue electroluminescent fiber. The electroluminescent spectrum is shown in Figure 2 As shown by arrow 4, the CIE color coordinates are Figure 3 As shown in the middle circle A.

[0067] Example 4

[0068] Step 1: Preparation of nano quantum dots as light-converting particles: 0.4 mmol PbBr2 and 0.4 mmol CsBr were dissolved in 10 mL DMF. 1 mL OA and 1 mL APTES were added to stabilize the precursor solution. Then, 1 mL of the precursor solution was quickly added to 10 mL toluene under vigorous stirring to obtain CsPbBr3 quantum dots (particle size 8 nm, emitting green light).

[0069] Step 2: Preparation of a novel electroluminescent active material modified by nano-quantum dot grafting: Take 2 mL of CsPbBr3 nano-quantum dot solution, add 5 μL of APTES, ultrasonicate and stir for 1 hour, add 0.5 g of ZnS, 5 μL of APTES, 5 μL of deionized water, and stir at 45 ° C for 24 hours. Collect the precipitate by centrifugation, wash it three times with toluene, and dry it under vacuum to obtain a novel electroluminescent active material ZnS-g-CsPbBr3 (particle size 3.5 μm, emitting green light) modified by nano-quantum dot grafting.

[0070] Step 3: Loading the luminescent active layer: Take 1g of polyurethane and 3g of the new electroluminescent active material, mix them evenly at room temperature to obtain a uniformly dispersed luminescent layer slurry. The active luminescent slurry is coated on the surface of a copper wire with a diameter of 100μm through a 160μm limiting hole at a coating speed of 0.8m / min, and then heated and cured at 60°C to obtain a conductive fiber loaded with a luminescent active layer.

[0071] Step 4: Loading the external electrode: Turn on the twisting device and load the silver fiber (diameter 80μm) on the fiber in step 3 with a pitch of 0.5mm and a twisting speed of 2m / min to obtain a high color purity green electroluminescent fiber. Its electroluminescent spectrum is as follows Figure 2 As shown by arrow 5, the CIE color coordinates are Figure 3 As shown in the middle circle B.

Claims

1. A method for preparing high color purity multi-color electroluminescent fiber, characterized in that: The specific steps are as follows: (1) Preparation of quantum dot light conversion particles: Preparation of lead halide perovskite nano-quantum dots CsPbX3 QDs as light conversion particles by hot injection or room temperature supersaturated recrystallization; (2) Preparation of electroluminescent active materials modified with light-converting particles: Lead halide perovskite nano-quantum dots are grafted onto the surface of metal sulfide electroluminescent particles through surface ligands to obtain high color purity multi-color electroluminescent active materials; the color of the electroluminescent active materials can be directionally controlled by changing the type and ratio of halogen in the perovskite nano-quantum dot material; The types of halogen in the perovskite nano-quantum dots are Cl, Br, and I, and the size of the perovskite nano-quantum dots is 5-20 nm; (3) Loading the luminescent active layer: Compounding the electroluminescent active material modified by the light conversion particles and the transparent thermoplastic elastomer polymer to obtain a uniform and stable luminescent active slurry, and coating the luminescent active slurry on the surface of the conductive fiber through a continuous confined coating process to obtain a conductive fiber coated with the electroluminescent active layer; (4) Loading fiber external electrode: The external electrode is loaded on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain high color purity multi-color electroluminescent fiber, and the luminescent colors are pure red, orange, yellow, green, blue, purple, and white.

2. The preparation method according to claim 1, characterized in that: In step (1): The specific steps of the hot injection method are: 0.276-0.4 g Cs2CO3, 10-15 mL octadecene (ODE) and 0.833-1.76 mL surface ligand are selected, mixed and stirred, and placed in a three-necked flask, heated to 120-140° C. under N2 atmosphere and dried for 0.5-1 hour to obtain a cesium oleate precursor solution; 0.376-0.752mmol PbX2 (X = Cl, Br, I) and 10-20mL ODE were placed in a 100mL flask, heated to 120-140°C under N2 atmosphere and dried for 0.5-1 hour; then, 1-2mL of surface ligand was slowly injected into the flask under stirring, and stirred until the solution became clear; the flask was heated to 160-180°C, and 0.8-1.6mL of cesium oleate precursor solution was quickly injected, and after standing for 5-10s, the mixture solution was cooled to room temperature using an ice water bath; it was washed with an antisolvent and redispersed in 1-2mL of toluene or n-hexane for further use; The specific steps of the room temperature supersaturated recrystallization method are: Dissolve 0.4-0.8mmol PbX2 and 0.4-0.8mmol CsX (X=Cl, Br, I) in 10mL DMF or DMSO, add 1mL surface ligand to stabilize the precursor solution; then, under vigorous stirring, quickly add 0.5-1mL precursor solution into 10mL toluene.

3. The preparation method according to claim 2, characterized in that: In the hot injection method, the surface ligand is a mixture of one or more of oleic acid OA, oleylamine OAm, 3-aminopropyltriethoxysilane APTES, and trioctylphosphine TOP; the anti-solvent is ethyl acetate or methyl acetate; In the room temperature supersaturated recrystallization method, the surface ligand is a mixture of one or more of oleic acid OA, oleylamine OAm, and 3-aminopropyltriethoxysilane APTES.

4. The preparation method according to claim 1, characterized in that: In step (2), the grafting modification method includes two methods, specifically: Method 1: 0.5-1g of electroluminescent particles are mixed with 2mL of perovskite nanocrystal solution, 2-5μL of deionized water is added, and the mixture is stirred at 60-80°C for 24-30 hours; then, 5-20μL of silane coupling agent and 2-5μL of deionized water are added, and the mixture is stirred at 60-80°C for 6-8 hours; the precipitate is collected by centrifugation, and washed three times with toluene; and dried under vacuum to obtain an electroluminescent active material modified with nano-quantum dots; or: Method 2: Add 5 μL of silane coupling agent to 2 mL of perovskite nanocrystal solution, sonicate and stir for 1 hour; add 0.5-1.2 g of electroluminescent particles, 5-10 μL of silane coupling agent and 2-5 μL of deionized water, stir at 45°C for 24-32 hours; collect the precipitate by centrifugation, wash it with toluene three times; dry it under vacuum to obtain the electroluminescent active material modified with nano-quantum dots; When the hot injection method is used in step (1), the grafting modification method in step (2) is method 1 or method 2; When the room temperature supersaturated recrystallization method is used in step (1), the grafting modification method in step (2) is method 2.

5. The preparation method according to claim 4, characterized in that: The electroluminescent particles are CaS, SrS or ZnS; The silane coupling agent is 3-aminopropyltriethoxysilane APTES, γ-mercaptopropyltriethoxysilane MPTES or γ-mercaptopropyltrimethoxysilane MPTMS.

6. The preparation method according to claim 5, characterized in that: The particle size of the obtained nano-quantum dot-modified electroluminescent active material is 0.5-5 μm.

7. The preparation method according to claim 1, characterized in that: In step (3): The conductive fiber is a metal conductive fiber, an ion gel fiber or a conductive polymer composite fiber; The transparent thermoplastic elastomer polymer is polyester polyurethane, fluororubber or thermoplastic polyolefin elastomer; The conductive fiber has a diameter of 50-120 μm; the conductive fiber has a resistance of 5-50 Ω / m; The coating thickness of the electroluminescent active layer is 10-50 μm; the coating process is specifically: dipping and heating curing, the dipping speed is 0.1-1 m / min, and the heating temperature is 60-100°C.

8. The preparation method according to claim 1, characterized in that: In step (4), the external electrode is a metal wire, specifically selected from one of copper wire, silver wire, stainless steel wire and aluminum wire; the diameter of the metal wire is 30-80 μm, and the resistance is 0.5-50 Ω / m; The twisting or twisting process is specifically as follows: the pitch is 0.1-2 mm and the speed is 1-10 m / min.

9. The high color purity multi-color electroluminescent fiber obtained by the preparation method according to any one of claims 1 to 8, wherein the luminescent fiber comprises, from inside to outside: Conductive fibers, luminescent active layer, and external electrode form an electrode-luminescent layer-electrode, i.e., a "sandwich" structure; The diameter of the luminous fiber is 0.20-0.25 mm, and the luminous brightness is 30-60 cd / m 2 The luminous colors include pure red, orange, yellow, green, blue, purple and white, with high color purity.

10. The use of the high color purity multi-color electroluminescent fiber as claimed in claim 9 as clothing material in the production of clothing by weaving, embroidery and knitting.

Citation Information

Patent Citations

  • High-elasticity electroluminescent fiber and preparation method thereof

    CN108093535A

  • Stable organic light emitting coating

    CN111670215A

  • White light electroluminescent fiber and preparation method thereof

    CN117626634A

  • Light-emitting device, preparation method thereof and display device

    CN118201439A

  • Composite material, photoelectric device, and preparation method therefor

    WO2024067203A1