Black ruthenium plating solution and its application in the preparation of antique gold or platinum jewelry

By using special black ruthenium plating solution and magnetorheological polishing technology on precious metals, the problem of poor aging effect in the existing technology is solved, and a dark, uniform and environmentally friendly retro effect is achieved, and the recycling of precious metals is supported. .

CN115787010BActive Publication Date: 2024-11-12CHOW TAI FOOK JEWELRY CULTURAL IND PARK WUHAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211540845.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-11-12
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The prior art is not dark enough when making precious metals such as gold and platinum, and poor uniformity and mechanical properties. Traditional black ruthenium electroplating lacks retro aging effect, and environmentally friendly and waste recycling is not good.

Method used

A black ruthenium plating solution is used, containing the ruthenium complex in the form of [Ru(bpy)2]a[Ru(en)3]c, a halogen anionic salt, sulfur-containing compound blackening agent and sacrificial oxidant, pH ≤3, combined with Magnetic rheology polishing technology, performs the aging treatment of retro precious metals.

Benefits of technology

It has achieved improvements in the depth, uniformity and mechanical properties of the black coating, with a unique retro flavor, and is environmentally friendly, without producing hazardous waste, and supports the recycling and reuse of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115787010B_ABST
    Figure CN115787010B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of jewelry preparation technology, in particular to a black ruthenium plating solution and its application in the preparation of vintage gold or platinum jewelry. The black ruthenium plating solution contains: a) [Ru(bpy)2] a [Ru(en)3] b [Ru2N(H2O)2X3] c a) a ruthenium complex in the form of a black ruthenium plating solution; wherein X is a halogen anion and its concentration in terms of Ru is 0.02M to 0.1M; b) a salt of a halogen anion with a concentration of 0.001M to 1M; c) a sulfur-containing compound present as a blackening agent; and d) a sacrificial oxidant; wherein the pH of the black ruthenium plating solution is ≤3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of jewelry preparation technology, and in particular to a black ruthenium plating solution and an application thereof in the preparation of vintage gold, platinum and other jewelry. Background Art

[0002] It is generally believed in the prior art that gold and platinum are generally not easy to age, and the degree of similarity of aging is low. The main reason is that gold and platinum are chemically stable and not easy to oxidize, and traditional sulfurization aging is not environmentally friendly. In addition, gold and platinum generally show reddish-brown spots when naturally oxidized, and will not show uniform and stable black lines. They are not aesthetically pleasing and cannot be produced in a standardized manner.

[0003] Ruthenium, as a light grey platinum group precious metal, is often used in functional and decorative electroplating due to its excellent corrosion resistance and wear resistance. "Black ruthenium" is commonly known as "black gold" because a blackening agent is added to the plating solution, so the ruthenium electroplating film can emit black. However, traditional black ruthenium electroplating also has problems such as insufficient color depth, poor uniformity of the coating, and poor mechanical properties due to the instability of the blackening agent. In addition, traditional black ruthenium electroplating has no research on retro aging effects.

[0004] A Chinese patent application with publication date of February 8, 2006 and publication number CN1729884A discloses a process for producing different color effects on the surface of a metal material after color separation electroplating. However, the method is not highly automated and does not describe grinding and polishing after electroplating ruthenium blackening.

[0005] A Chinese patent application with a publication date of March 5, 2008 and a publication number of CN101675185A discloses a formula of a phosphonic acid derivative black ruthenium plating solution. The formula is conventional and the plating effect is not ideal.

[0006] In general, existing aging technologies, such as silver aging, generally use sulfur boiling, which is not environmentally friendly, and the color is grayish, the film layer is not correct in color, and there is no sense of thickness, like a semi-finished product, and the aging process is poor. In addition, the existing aging technology has no research on 24K gold, platinum, and 18K gold. This type of gold and platinum products generally show reddish-brown spots when naturally oxidized, and will not show uniform and stable black lines. They are not aesthetically pleasing and cannot be produced in a standardized manner. The existing black ruthenium plating solution also has problems such as insufficient color depth, poor uniformity of the coating, and poor mechanical properties due to the instability of the blackening agent. In addition, there is no research on the retro aging effect in traditional black ruthenium electroplating. Summary of the invention

[0007] The present invention relates to a black ruthenium plating solution, which comprises: a) [Ru(bpy)2] a [Ru(en)3] b [Ru2N(H2O)2X3]c A ruthenium complex in the form of; wherein X is a halogen anion, and the concentration of Ru is 0.02M to 0.1M; b) a salt of a halogen anion with a concentration of 0.001M to 1M; c) a sulfur-containing compound present as a blackening agent; and d) a sacrificial oxidant;

[0008] Wherein, the pH value of the black ruthenium plating solution is ≤3.

[0009] The method also provides a method for preparing the black ruthenium plating solution as described above, comprising:

[0010] i) heating a ruthenium compound, a ligand, an auxiliary ligand and an aminosulfonic acid substance in excess relative to the ruthenium compound under acidic conditions to form a ruthenium complex;

[0011] Wherein, the ligand includes ethylenediamine and / or its salt, and pyridine derivative salt; the auxiliary ligand is one or more of ammonium citrate, nitrite, and sulfite;

[0012] ii) while maintaining the acidic and heated conditions, add the salt of the halogen anion, the blackening agent and the sacrificial oxidant to the process in i).

[0013] The present invention also provides a method for preparing vintage precious metals (especially vintage gold and vintage platinum), comprising the step of performing an aging treatment using the black ruthenium plating solution as described above.

[0014] The present invention further provides vintage precious metals (especially vintage gold and vintage platinum) and ornaments containing the same.

[0015] Compared with the prior art, the present invention provides a black ruthenium plating solution for a retro effect process for jewelry. The process based on the black ruthenium plating solution solves the problem that the black ruthenium coating has poor bonding with precious metals, especially gold and platinum, and has a gray color. And the process preferentially applies magnetorheological polishing technology to make the black ruthenium coating on the surface of gold and platinum into a retro and old effect. This effect makes the overall color of the product slightly darker, with black remaining in some positions, and the structure of the black remaining part is stable, the color is rich, the lines are clear, and it is full of layers and sense of age, showing a unique retro charm. This process product basically does not affect the color and weight of the product, and the precious metal waste generated in the production process is purified and recycled, no hazardous waste is generated, and it is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 This is a photo of an ornament prepared according to an embodiment of the present invention.

[0018] Figure 2 The following are photos of jewelry prepared according to an embodiment of the present invention; A uses the black ruthenium solution of the comparative example, which is grayish in color; B is the black ruthenium solution provided by the present invention, which is dark black in color.

[0019] Figure 3 The results of coating adhesion test; A is a comparative black ruthenium solution coating test piece, and B is a black ruthenium solution coating test piece provided by the present invention.

[0020] Figure 4 Graphs showing bending test results; A is a comparative black ruthenium solution coating test piece, and B is a black ruthenium solution coating test piece provided by the present invention. DETAILED DESCRIPTION

[0021] References to embodiments of the present invention will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present invention. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present invention without departing from the scope or spirit of the present invention. For example, a feature illustrated or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0022] Unless otherwise indicated, the meaning of all terms (including technical and scientific terms) used to disclose the present invention is the same as that commonly understood by those of ordinary skill in the art to which the present invention belongs. By way of further guidance, the following definitions are used to better understand the teachings of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0023] The terms "and / or", "or / and", and "and / or" used in this article include any one of two or more related listed items, and also include any and all combinations of related listed items, and the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in this application, the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution that is all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four of A, B, C, and D (that is, the technical solution that is all connected by "logical AND").

[0024] As used herein, the terms "comprising", "including" and "comprising" are synonymous and are inclusive or open-ended and do not exclude additional, unrecited members, elements or method steps.

[0025] Numerical ranges expressed as endpoints herein include all numbers and fractions subsumed within the range, as well as the recited endpoints.

[0026] The present invention relates to concentration values, and its meaning includes fluctuations within a certain range. For example, it can fluctuate within the corresponding accuracy range. For example, 2% can allow fluctuations within the range of ±0.1%. For values ​​that are large or do not require too fine control, its meaning is also allowed to include greater fluctuations. For example, 100mM can allow fluctuations within the range of ±1%, ±2%, ±5%, etc. Involving molecular weight, its meaning is allowed to include fluctuations of ±10%.

[0027] In the present invention, descriptions such as "plurality" and "multiple" refer to quantities greater than or equal to 2 unless otherwise specified.

[0028] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0029] In the present invention, "preferably", "better", "more preferably", and "suitably" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. In the present invention, "optionally", "optional", and "optional" refer to being optional, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent of each other.

[0030] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as a reference separately. Unless they conflict with the invention purpose and / or technical solution of the present application, the cited documents involved in the present invention are cited with all contents and all purposes. When the present invention involves cited documents, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the present invention involves cited documents, the examples and preferred embodiments of the cited relevant technical features may also be incorporated into this application as references, but are limited to the ability to implement the present invention. It should be understood that when the content of the citation conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.

[0031] The present invention relates to a black ruthenium plating solution, which comprises: a) [Ru(bpy)2] a [Ru(en)3] b [Ru2N(H2O)2X3] c A ruthenium complex in the form of; wherein X is a halogen anion, and the concentration of Ru is 0.02M to 0.1M; b) a salt of a halogen anion with a concentration of 0.001M to 1M; c) a sulfur-containing compound present as a blackening agent; and d) a sacrificial oxidant;

[0032] Wherein, the pH value of the black ruthenium plating solution is ≤3.

[0033] bpy is a pyridine group, and en is an ethylenediamine group.

[0034] a, b, c are non-zero positive integers.

[0035] The pH of the black ruthenium plating solution is preferably 0.5 to 2.5.

[0036] The concentration of component a) in terms of Ru may also be 0.05M or 0.07M.

[0037] b) The concentration of the halogen anion can also be 0.005M, 0.01M, 0.05M, 0.1M, or 0.5M.

[0038] The solvent of the black ruthenium plating solution can be double distilled water, deionized water or ultrapure water.

[0039] In some embodiments, the cation of the salt of the halide anion is an ammonium ion.

[0040] When the cation is an ammonium ion (such as ammonium chloride, ammonium bromide, ammonium iodide, etc.), these components can be used as brighteners at the same time, so there is no need to add brighteners additionally.

[0041] In some embodiments, the sacrificial oxidant is one or more of ascorbic acid, hydroxylamine sulfate, sodium hexametaphosphate, or trisodium phosphate.

[0042] The added amount of the sacrificial oxidant may be 0.01M to 5M, for example 0.05M, 0.1M, 0.5M, 1M, 3M.

[0043] In some embodiments, the sulfur-containing compound includes one or more of thiomalic acid, thioglycolic acid, β-mercaptopropionic acid, thiourea, ammonium thiocyanate, and thiourea derivatives.

[0044] The added amount of the blackening agent can be 0.01M to 10M, for example, 0.05M, 0.1M, 0.5M, 1M, 3M, 5M, 7M.

[0045] In some embodiments, the black ruthenium plating solution contains a brightener, which can be used as an auxiliary coloring agent to improve the flatness and flexibility of the black ruthenium coating.

[0046] The added amount of the brightener can be 0.01M to 10M, for example, 0.05M, 0.1M, 0.5M, 1M, 3M, 5M, 7M.

[0047] Furthermore, the brightener is selected from one or more of methyl ammonium iodide, sodium xylene sulfonate, ammonium chloride, magnesium sulfate and ammonium bromide.

[0048] In some embodiments, the concentration of the black ruthenium plating solution is 2°Bé to 25°Bé, for example, 5°Bé, 10°Bé, 15°Bé, or 20°Bé.

[0049] In some embodiments, the halogen anion is Cl - Br - ,I - At least one of .

[0050] In some embodiments, the black ruthenium plating solution has a color number of Black 6C.

[0051] According to another aspect of the present invention, it also relates to a method for preparing the black ruthenium plating solution as described above, comprising:

[0052] i) heating a ruthenium compound, a ligand, an auxiliary ligand and an aminosulfonic acid substance in excess relative to the ruthenium compound under acidic conditions to form a ruthenium complex;

[0053] Wherein, the ligand includes ethylenediamine and / or its salt, and pyridine derivative salt; the auxiliary ligand is one or more of ammonium citrate, nitrite, and sulfite;

[0054] ii) while maintaining the acidic and heated conditions, add the salt of the halogen anion, the blackening agent and the sacrificial oxidant to the process in i).

[0055] In some embodiments, the ruthenium compound includes one or more of ruthenium trichloride, ruthenium sulfate, ruthenium nitrosyl sulfate, and ruthenium sulfamate.

[0056] In some embodiments, the heating temperature is 60°C to 80°C, such as 65°C, 70°C, or 75°C.

[0057] According to another aspect of the present invention, there is also a method for preparing vintage precious metals, comprising the step of performing an aging treatment using the black ruthenium plating solution as described above.

[0058] The preparation method of vintage precious metals may be known to those skilled in the art, such as the method previously disclosed by the applicant in CN110965088A and CN113774435A.

[0059] In some embodiments, the preparation method comprises:

[0060] 1) forming a noble metal mold and electroplating it with the black ruthenium plating solution;

[0061] 2) Remove the black plating of the precious metal mold and polish it;

[0062] 3) The polished precious metal is treated with acid, and then molded and polished again.

[0063] In some embodiments, the electroplating treatment conditions are: the plating solution temperature is 30°C to 70°C, the cathode current density is 0.3A / dm 2 ~10.0A / dm 2 , electroplating time is 3 to 30 minutes.

[0064] The workpiece swings preferably at 10 to 60 revolutions per minute during the electroplating process.

[0065] In some embodiments, the acid used in the acid treatment is one or more of sulfuric acid (preferably 98% sulfuric acid), hydrochloric acid, and nitric acid, and the acid treatment temperature is 80 to 130° C. and the time is 5 to 20 seconds.

[0066] In some embodiments, the mold removal is specifically to leave a black line on the concave lines and seams, and rub off the black parts with 800-1200# sandpaper in the rest of the places. Further preferably, the convex parts of the product are polished using a polishing agent and a magnetic polishing material in a polishing machine, and the polishing time is preferably 5min to 60min, for example, 10min, 20min, 30min, 40min, 50min. The polishing machine can be one or more of a magnetic needle polishing machine, a ball polishing machine, or a magnetorheological polishing machine.

[0067] In some embodiments, the polishing comprises magnetic polishing, preferably magnetorheological polishing, and more preferably a 3-axis magnetorheological polisher.

[0068] In some embodiments, the magnetorheological polishing conditions include: magnetic field strength of 60% to 85%, spindle speed of 50 r / min to 120 r / min, and polishing time of 15 min to 30 min.

[0069] In some embodiments, the polishing agent is one or more of ethyl acetate, butyl acetate, ethylene glycol, aluminum oxide, and silicon dioxide.

[0070] In some embodiments, the magnetic polishing material is one or more of magnetic needles, magnetic beads, magnetic sand, atomized iron powder, and carbonyl iron powder.

[0071] In some embodiments, the method further comprises the step of recycling and purifying the precious metal waste.

[0072] The precious metal recovery and purification generally includes targeted material adsorption (the targeted material generally includes one or more of cellulose ethylenediamine, mercaptopolyethylene glycol silicon, methyl mercaptan polystyrene), desorption, precipitation reduction, and precious metal smelting and then reuse in the production line.

[0073] In some embodiments, the precious metal is gold and / or platinum.

[0074] The gold may be 24K gold, 18K gold, etc.

[0075] The present invention also relates to the vintage precious metal prepared by the method as described above.

[0076] According to yet another aspect of the present invention, there is also provided an ornament comprising the antique precious metal as described above.

[0077] In the present invention, "accessories" refers to all decorative items, such as jewelry and home accessories. Jewelry is preferred, such as accessories worn on the head, such as hairpins, hairpins, earrings, etc.; accessories worn on the body, such as necklaces, brooches, bracelets, rings, anklets, etc.; and can also be expensive pens, watches, knives, nameplates, etc.

[0078] Jewelry may also contain other decorative materials, typically such as platinum, gold, silver, gemstones.

[0079] Jewelry can contain one or more vintage precious metals, such as both vintage gold and vintage platinum.

[0080] The gemstones defined in the present invention are broad in scope, including natural mineral crystals, such as diamond, crystal, emerald, ruby, sapphire, chrysoberyl (alexandrite, cat's eye), epidote, etc.; there are also a few natural single mineral aggregates, such as ulanzan and opal. There are also a few organic materials, such as amber, pearl, coral, and jet, which are also included in the broad definition of gemstones.

[0081] Embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are preferably referred to the guidance provided in the present invention, and can also be based on the experimental manual or normal conditions in this area, and can also be based on other experimental methods known in the art, or according to the conditions recommended by the manufacturer.

[0082] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0083] Example 1 Preparation of black ruthenium plating solution

[0084] 1. Select ruthenium trichloride or ruthenium sulfate as the ruthenium source of the plating solution, dissolve 0.05 mol of ruthenium compound (ruthenium mass fraction 30%-60%) in 1L ultrapure water to obtain solution A, and the detected ruthenium concentration is about 0.02 mol / L.

[0085] 2. Add 1 mol of ethylenediamine, 0.03 mol of 2,2'-bipyridine, 0.01 mol of arylaminosulfonic acid, and 0.015 mol of sodium nitrite to solution A, reflux for 5 h, and then perform post-treatment such as precipitation, filtration, and aging reaction to obtain a series of products containing the structural formula [Ru(bpy)2] a [Ru(en)3] b [Ru2N(H2O)2Cl3] c The ruthenium mixed ligand complex B has special stability due to the formation of a cyclic chelate structure.

[0086] 3. When preparing the plating solution, dilute the above complex B with ultrapure water to a concentration of 0.05 mol / L in terms of Ru. Add sulfuric acid, sulfate or aminosulfonate to the plating solution at a concentration of about 1 mol / L and stir at 70°C for 1 hour to improve the stability of the ruthenium electroplating solution.

[0087] 4. Add halogen anion compounds to increase the deposition rate of ruthenium. Appropriate concentrations can produce crack-free ruthenium coatings and improve the brightness and mechanical strength of ruthenium coatings. Suitable halogen anions are Cl - and Br - When preparing the plating solution, add ammonium chloride and ammonium bromide, the concentration of which is about 0.5 mol / L, stir at 70°C for 2 hours to obtain plating solution C.

[0088] 5. Add 0.01-10 mol / L β-mercaptopropionic acid, thiourea derivatives, and other thiol-containing compounds to the plating solution C. The thiol compounds and complex B can play a role in blackening. Then add 3 mol / L hydroxylamine sulfate and sodium hexametaphosphate to enhance the antioxidant properties of the plating solution C and stabilize the blackness of the ruthenium coating. After adding the above additives, stir at 70°C for 3 hours, adjust the pH to <3, and obtain the final product plating solution D.

[0089] 6. During electroplating, keep the plating solution D at 60-70°C with strong mechanical stirring. The appropriate current density is 5-10ASD. Too high or too low current density will affect the blackness and bonding strength of the coating. In addition, when working with the plating solution, you need to pay extra attention to the solution concentration. Generally, 2-25°Bé is more appropriate. Too high a solution concentration will lead to poor coating quality and increase the consumption of chemicals.

[0090] Example 2 Preparation of black ruthenium plating solution

[0091] 1. Select ruthenium trichloride or ruthenium sulfate as the ruthenium source of the plating solution, dissolve 0.05 mol of ruthenium compound (ruthenium mass fraction 30%-60%) in 1L ultrapure water to obtain solution A, and the detected ruthenium concentration is about 0.05 mol / L.

[0092] 2. Add 0.05 mol ethylenediamine, 0.06 mol 2,2'-bipyridine, 0.005 mol arylaminosulfonic acid, and 0.03 mol sodium nitrite to solution A, reflux for 4 h, and then perform post-treatment such as precipitation, filtration, and aging reaction to obtain a series of products containing the structural formula [Ru(bpy)2] a [Ru(en)3] b [Ru2N(H2O)2Cl3] c The ruthenium mixed ligand complex B has special stability due to the formation of a cyclic chelate structure.

[0093] 3. When preparing the plating solution, dilute the above complex B with ultrapure water to a concentration of 0.02 mol / L in terms of Ru. Add sulfuric acid, sulfate or aminosulfonate to the plating solution at a concentration of about 0.05 mol / L and stir at 70°C for 1 hour to improve the stability of the ruthenium electroplating solution.

[0094] 4. Add halogen anion compounds to increase the deposition rate of ruthenium. Appropriate concentrations can produce crack-free ruthenium coatings and improve the brightness and mechanical strength of ruthenium coatings. Suitable halogen anions are Cl - When preparing this plating solution, add ammonium chloride with a concentration of about 0.01 mol / L, stir at 70°C for 2 hours to obtain plating solution C.

[0095] 5. Add 0.1 mol / L β-mercaptopropionic acid, thiourea derivatives and other thiol-containing compounds to the plating solution C. The thiol compounds and complex B can play a role in blackening. Then add 5 mol / L hydroxylamine sulfate and sodium hexametaphosphate to enhance the antioxidant property of the plating solution C and stabilize the blackness of the ruthenium coating. After adding the above additives, stir at 70°C for 3 hours, adjust the pH to <3, and obtain the final product plating solution D.

[0096] 6. During electroplating, keep the plating solution D at 60-70°C with strong mechanical stirring. The appropriate current density is 5-10ASD. Too high or too low current density will affect the blackness and bonding strength of the coating. In addition, when working with the plating solution, you need to pay extra attention to the solution concentration. Generally, 2-25°Bé is more appropriate. Too high a solution concentration will lead to poor coating quality and increase the consumption of chemicals.

[0097] Example 3 Preparation of black ruthenium plating solution

[0098] 1. Select ruthenium trichloride or ruthenium sulfate as the ruthenium source of the plating solution, dissolve 0.05 mol of ruthenium compound (ruthenium mass fraction 30%-60%) in 1L of ultrapure water to obtain solution A, and the detected ruthenium concentration is about 0.1 mol / L.

[0099] 2. Add 2 mol of ethylenediamine, 0.02 mol of 2,2'-bipyridine, 0.02 mol of arylaminosulfonic acid, and 0.01 mol of sodium nitrite to solution A, reflux for 7 h, and then obtain a series of products containing the structural formula [Ru(bpy)2] by post-treatment such as precipitation, filtration, and aging reaction. a [Ru(en)3] b [Ru2N(H2O)2Cl3] c The ruthenium mixed ligand complex B has special stability due to the formation of a cyclic chelate structure.

[0100] 3. When preparing the plating solution, dilute the above complex B with ultrapure water to a concentration of 0.1 mol / L in terms of Ru. Add sulfuric acid, sulfate or aminosulfonate to the plating solution at a concentration of about 2 mol / L and stir at 70°C for 1 hour to improve the stability of the ruthenium electroplating solution.

[0101] 4. Add halogen anion compounds to increase the deposition rate of ruthenium. Appropriate concentrations can produce crack-free ruthenium coatings and improve the brightness and mechanical strength of ruthenium coatings. Appropriate halogen anions are Br - When preparing the plating solution, ammonium bromide was added at a concentration of about 1 mol / L, and the temperature was 70°C and stirred for 2 hours to obtain plating solution C.

[0102] 5. Add 10 mol / L β-mercaptopropionic acid, thiourea derivatives, and other thiol-containing compounds to the plating solution C. The thiol compounds and complex B can play a role in blackening. Then add 0.01 mol / L hydroxylamine sulfate and sodium hexametaphosphate to enhance the antioxidant properties of the plating solution C and stabilize the blackness of the ruthenium coating. After adding the above additives, stir at 70°C for 3 hours, adjust the pH to <3, and obtain the final product plating solution D.

[0103] 6. During electroplating, keep the plating solution D at 60-70°C with strong mechanical stirring. The appropriate current density is 5-10ASD. Too high or too low current density will affect the blackness and bonding strength of the coating. In addition, when working with the plating solution, you need to pay extra attention to the solution concentration. Generally, 2-25°Bé is more appropriate. Too high a solution concentration will lead to poor coating quality and increase the consumption of chemicals.

[0104] Example 4 Black ruthenium plating solution and its application in retro jewelry

[0105] The overall steps of preparing vintage jewelry can be referred to Chinese patent applications CN110965088A and CN113774435A, which are generally described as follows:

[0106] Step 1: Make the gold and platinum blanks into molds;

[0107] Step 2: prepare an ultra-dark black ruthenium plating solution (see Examples 1 to 3);

[0108] Step 3: Electroplating the gold and platinum after molding with ultra-deep black ruthenium;

[0109] Step 4: Perform surface treatments such as mold removal and magnetic polishing on the black-plated gold and platinum.

[0110] Step 5: acid-treating, molding, inlaying, assembling and polishing the surface-treated gold and platinum to obtain the product;

[0111] Step 6: Recycle the waste precious metals generated in this process, purify them and reuse them in production.

[0112] Some details have been improved as follows:

[0113] The conditions for ultra-deep black ruthenium electroplating may generally include: a plating solution temperature of 30-70°C, a plating solution pH of 0.5-2.5, a cathode current density of 0.3-10.0 A / dm2, a plating time of 3-30 minutes, and a workpiece swing of 10-60 revolutions per minute.

[0114] The mold removal and polishing are to rub off the black part with 800-1200# sandpaper, and polish the raised part of the product with a polishing agent and a magnetic polishing material in a polishing machine, and the polishing time is 5-60 minutes; the polishing machine is one or more of a magnetic needle polishing machine, a ball polishing machine or a magnetorheological polishing machine.

[0115] The exemplary pictures of the products prepared therefrom are as follows Figure 1 shown.

[0116] Experimental example

[0117] The black ruthenium plating solution of Example 1 was used for testing. When jewelry was prepared, the method of Example 4 was used. The comparative example used an externally purchased black ruthenium plating solution produced by Germany (Umekohl), the publication date of the patent corresponding to its product was September 10, 2014, and the authorization announcement number was CN104040033B. Except for the different black ruthenium plating solutions and electroplating parameters (the electroplating parameters of the comparative example adopted the parameters recommended by commercial products), other parameters were the same.

[0118] 1. Blackness detection

[0119] The color spectrum spectrophotometer DS-700D is used to test the blackness of black ruthenium coating. The principle of color measurement is: use ultraviolet and LED light sources to project objects to measure the reflectivity, and obtain three parameters: L (black-white), a (green-red), and b (blue-yellow). The smaller the L (black-white) number, the blacker it is; the smaller the a (green-red) number, the greener it is; and the smaller the b (blue-yellow) number, the bluer it is.

[0120] Experimental Procedure

[0121] First turn on the device, place the instrument on the calibration base for white calibration, and then align the instrument with the air for black calibration. After calibration, switch the device to the appropriate aperture and select the corresponding mode according to the aperture. Place the electroplated black ruthenium sample on the bottom of the colorimeter, click Start, and start measuring.

[0122] The ornaments prepared by different groups are as follows Figure 2 The test results are shown in Table 1.

[0123] Table 1

[0124]

[0125] In Table 1, the L value of the self-made black ruthenium solution is 35.34, which is less than the L value of the purchased black ruthenium solution 41.03, indicating that the self-made black ruthenium solution coating is darker and Figure 2 It can also be clearly seen by visual inspection that the color of the independent black ruthenium coating is darker and blacker.

[0126] 2. Binding strength test

[0127] ⑴ Coating adhesion test

[0128] Experimental Procedure

[0129] The experimental piece was electroplated with black ruthenium film, and the process parameters were: current density 5ASD, temperature 65℃, electroplating time 5min. After electroplating, the experimental piece was fixed on the fixture, and 3M adhesive tape was attached to the surface of the electroplated layer. An eraser was used to rub it back and forth to make it completely fit, and then it was quickly torn off in a 45° direction.

[0130] The experimental results are as follows Figure 3 As shown. Figure 3 It can be seen that through visual observation, the self-produced black ruthenium solution coating has no fading, peeling, or blistering, while the purchased black ruthenium solution coating has obvious coating peeling and fading.

[0131] ⑵Bending test

[0132] Experimental Procedure

[0133] The experimental piece was electroplated with a black ruthenium film, and the electroplating process was as follows: current density 5ASD, temperature 65°C, and electroplating time 5min. After electroplating, the experimental piece was fixed on a fixture and bent at 90°, and then the bent surface was observed with a 10x microscope.

[0134] Depend on Figure 4 It can be seen that through visual observation, the self-produced black ruthenium solution coating has no fading, peeling, or blistering, while the purchased black ruthenium solution coating has obvious coating peeling and fading on the curved surface.

[0135] In summary, the black ruthenium plating solution provided by the present invention has significantly better blackness and bonding strength than commercially available products.

[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.

Claims

1. A black ruthenium plating solution comprising: a) a ruthenium complex; b) a salt of a halogen anion with a concentration of 0.001M to 1M; c) a sulfur-containing compound present as a blackening agent; and d) a sacrificial oxidant; in, The pH of the black ruthenium plating solution is ≤3; The black ruthenium plating solution is prepared by the following preparation method: i) heating a ruthenium compound, ruthenium trichloride, a ligand in excess relative to the ruthenium compound, an auxiliary ligand and an arylaminosulfonic acid under reflux under acidic conditions to form a ruthenium complex; Wherein, the ligand is ethylenediamine and 2,2'-bipyridine; the auxiliary ligand is sodium nitrite; Wherein, the concentration of ruthenium trichloride calculated as Ru is 0.02 mol / L, the concentration of ethylenediamine is 1 mol / L, the concentration of 2,2'-bipyridine is 0.03 mol / L, the concentration of arylaminosulfonic acid is 0.01 mol / L, and the concentration of sodium nitrite is 0.015 mol / L; or the concentration of ruthenium trichloride calculated as Ru is 0.05 mol / L, the concentration of ethylenediamine is 0.05 mol / L, the concentration of 2,2'-bipyridine is 0.06 mol / L, the concentration of arylaminosulfonic acid is 0.005 mol / L, and the concentration of sodium nitrite is 0.003 mol / L; or the concentration of ruthenium trichloride calculated as Ru is 0.1 mol / L, the concentration of ethylenediamine is 2 mol / L, the concentration of 2,2'-bipyridine is 0.02 mol / L, the concentration of arylaminosulfonic acid is 0.02 mol / L, and the concentration of sodium nitrite is 0.01 mol / L; ii) while maintaining the acidic and heated conditions, add the salt of the halogen anion, the blackening agent and the sacrificial oxidant to the process in i). 2 . The black ruthenium plating solution according to claim 1 , wherein the cation of the salt of the halogen anion is an ammonium ion.

3. The black ruthenium plating solution according to claim 1, wherein the sacrificial oxidant is one or more of ascorbic acid, hydroxylamine sulfate, sodium hexametaphosphate or trisodium phosphate.

4. The black ruthenium plating solution according to claim 1, wherein the sulfur-containing compound comprises one or more of thiomalic acid, thioglycolic acid, β-mercaptopropionic acid, thiourea, ammonium thiocyanate, and thiourea derivatives.

5. The black ruthenium plating solution according to any one of claims 1 to 4, comprising a brightener, wherein the brightener is selected from one or more of methyl ammonium iodide, sodium xylene sulfonate, ammonium chloride, magnesium sulfate and ammonium bromide.

6. The black ruthenium plating solution according to any one of claims 1 to 4, wherein the concentration is 2°Bé to 25°Bé.

7. The black ruthenium plating solution according to any one of claims 1 to 4, wherein the halogen anion is Cl - Br - ,I - At least one of .

8. The black ruthenium plating solution according to any one of claims 1 to 4, which has a color number of Black 6 C.

9. The method for preparing the black ruthenium plating solution according to any one of claims 1 to 8, comprising: i) heating a ruthenium compound, ruthenium trichloride, a ligand in excess relative to the ruthenium compound, an auxiliary ligand and an arylaminosulfonic acid under reflux under acidic conditions to form a ruthenium complex; Wherein, the ligand is ethylenediamine and 2,2'-bipyridine; the auxiliary ligand is sodium nitrite; Wherein, the concentration of ruthenium trichloride calculated as Ru is 0.02 mol / L, the concentration of ethylenediamine is 1 mol / L, the concentration of 2,2'-bipyridine is 0.03 mol / L, the concentration of arylaminosulfonic acid is 0.01 mol / L, and the concentration of sodium nitrite is 0.015 mol / L; or the concentration of ruthenium trichloride calculated as Ru is 0.05 mol / L, the concentration of ethylenediamine is 0.05 mol / L, the concentration of 2,2'-bipyridine is 0.06 mol / L, the concentration of arylaminosulfonic acid is 0.005 mol / L, and the concentration of sodium nitrite is 0.003 mol / L; or the concentration of ruthenium trichloride calculated as Ru is 0.1 mol / L, the concentration of ethylenediamine is 2 mol / L, the concentration of 2,2'-bipyridine is 0.02 mol / L, the concentration of arylaminosulfonic acid is 0.02 mol / L, and the concentration of sodium nitrite is 0.01 mol / L; ii) while maintaining the acidic and heated conditions, add the salt of the halogen anion, the blackening agent and the sacrificial oxidant to the process in i).

10. The preparation method according to claim 9, wherein the heating temperature is 60°C to 80°C.

11. A method for preparing vintage precious metals, comprising the step of using the black ruthenium plating solution described in any one of claims 1 to 8 for aging treatment.

12. The preparation method according to claim 11, comprising: 1) forming a precious metal mold and electroplating it with the black ruthenium plating solution; 2) Remove the black plating of precious metal molds and polish them; 3) The polished precious metal is treated with acid and then molded and polished again.

13. The preparation method according to claim 12, wherein the electroplating treatment conditions are: the plating solution temperature is 30°C to 70°C, the cathode current density is 0.3 A / dm 2 ~10.0 A / dm 2 , electroplating time is 3~30 minutes.

14. The preparation method according to claim 12, wherein the acid used in the acid treatment is one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the acid treatment temperature is 80-130°C and the time is 5-20s.

15. The preparation method according to claim 14, wherein the black removal of the mold is specifically to leave a black line on the concave lines and seams, and rub off the black parts of the rest with 800-1200# sandpaper. The preparation method according to claim 12 , wherein the polishing is magnetic polishing. The preparation method according to claim 16 , wherein the polishing is magnetorheological polishing.

18. The preparation method according to claim 17, wherein the conditions of the magnetorheological polishing include: a magnetic field strength of 60% to 85%, a spindle speed of 50 r / min to 120 r / min, and a polishing time of 15 min to 30 min.

19. The preparation method according to claim 12, further comprising the step of recovering and purifying precious metal waste.

20. The preparation method according to any one of claims 11 to 19, wherein the precious metal is gold and / or platinum.

21. The vintage precious metal prepared by the method according to any one of claims 11 to 20.

22. Jewelry comprising the vintage precious metal according to claim 21.