Laminated battery and preparation method thereof

By preparing a hole transport layer on the composite layer of the tandem battery and coating it with a filling layer, the problem of the textured structure composite layer not being covered is solved, the interface contact of the perovskite layer is improved, the buried defects are reduced, and the battery performance is improved. performance.

CN118870935APending Publication Date: 2024-10-29SHENZHEN PHENOSOLAR TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410885200.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

During the preparation process of the tandem battery, the composite layer of the textured structure is not completely covered by the self-assembled molecular layer, resulting in contact between the perovskite layer and the composite layer, causing carrier recombination problems and reducing device performance.

Method used

A hole transport layer is prepared on the composite layer of the bottom cell, and a filling material is coated on it to form a filling layer. The filling layer at least covers the positions on the composite layer that are not blocked by the hole transport layer, improving the interface contact of the perovskite layer and promoting Perovskite crystallizes and reduces perovskite buried interface defects.

Benefits of technology

The voltage and fill factor of the stacked cell are increased, and the performance of the photovoltaic module device is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118870935A_ABST
    Figure CN118870935A_ABST
Patent Text Reader

Abstract

The invention discloses a laminated cell and a preparation method thereof. The preparation method comprises the following steps: preparing the hole transport layer on the composite layer of the bottom cell; coating a filling material on the hole transport layer to form a filling layer, wherein the filling layer at least covers the position, which is not shielded by the hole transport layer, on the composite layer; and preparing other structures of the perovskite cell on the filling layer. The laminated cell is prepared by adopting a laminated cell preparation method, the laminated cell comprises a bottom cell and a perovskite cell which are connected, and a hole transport layer of the perovskite cell is provided with a filling material to form a filling layer. According to the invention, the hole transport layer of the perovskite cell is coated with the filling material to form the filling layer, and the filling layer can fill the position which is not covered by the hole transport layer, thereby effectively improving the interface contact of the perovskite layer, promoting the perovskite crystallization, reducing the defects of the perovskite buried interface, improving the voltage and filling factors of the assembled laminated cell, and improving the reliability of the cell. And the performance of the photovoltaic module device is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic and solar cell technology, and in particular to a laminated cell and a preparation method thereof. Background Art

[0002] In the photovoltaic field, the highest certified efficiency of heterogeneous crystalline silicon solar cells has reached 27.1%, close to its theoretical upper limit of 28.2%. In order to obtain higher efficiency, tandem cells can be prepared by stacking crystalline silicon cells with wide bandgap solar cells (such as perovskite cells). At present, the efficiency of two-terminal crystalline silicon / perovskite tandem cells has reached 33.9%, and there is still a lot of room for growth from the theoretical upper limit of 43% for two cells. High-efficiency two-terminal tandem cells require that the perovskite cells be processed on a velvet silicon substrate with a light-trapping structure, and the velvet size height on the silicon substrate is 700 nm~1000 nm. The processing order of perovskite cells in high-efficiency two-terminal tandem cells is usually self-assembled monolayer, perovskite layer, surface passivation layer, electron transport layer, buffer layer, transparent electrode, metal grid line and anti-reflection layer, among which the self-assembled monolayer is processed on the transparent electrode on the surface of the velvet silicon substrate, i.e., the composite layer, and then the perovskite layer is processed on it. However, it is still a challenge to achieve complete coverage of solution-processed self-assembled single molecules on the composite layer of the velvet structure. In the positions on the composite layer of the velvet structure that are not completely covered by the self-assembled molecular layer, there will be contact between the composite layer and the perovskite layer, leading to serious carrier recombination problems and further reducing device performance. Summary of the invention

[0003] Based on this, it is necessary to provide a method for preparing a laminated battery. The laminated battery preparation method of the present invention can improve the interface contact of the perovskite layer, promote perovskite crystallization, reduce the interface defects of the perovskite buried bottom, increase the voltage and fill factor of the laminated battery, and significantly improve the performance of the photovoltaic module device.

[0004] An embodiment of the present application provides a method for preparing a stacked battery.

[0005] A method for preparing a laminated battery comprises the following steps:

[0006] preparing a hole transport layer on the composite layer of the bottom cell;

[0007] Coating a filling material on the hole transport layer to form a filling layer, wherein the filling layer at least covers a position on the composite layer that is not shielded by the hole transport layer, wherein the filling material comprises an alkyl diamine salt, wherein the number of carbon atoms of the alkyl group in the cation of the alkyl diamine salt is less than 20, and the anion comprises a halogen ion, a sulfonate ion, a formate ion or a tetrafluoroborate ion; and

[0008] Other structures of the perovskite cell are prepared on the filling layer.

[0009] In some of the embodiments, the bottom cell includes a crystalline silicon cell or a thin film cell, the crystalline silicon cell includes a PERC cell (passivated emitter and back contact cell), a TOPCon cell (tunneling oxide passivation contact cell), an HJT cell (crystalline silicon heterojunction solar cell) or an IBC cell (back contact cell), and the thin film cell includes a GaAs cell (gallium arsenide cell), a CdTe cell (cadmium telluride cell) or a CIGS cell (copper indium gallium selenide cell).

[0010] In some embodiments, the laminated battery preparation method satisfies at least one of the following conditions:

[0011] (1) The hole transport layer comprises a single layer structure formed by a self-assembled material, or a double layer structure formed by nickel oxide and a self-assembled material, wherein the self-assembled material comprises one or more of 2PACz ([2-(9H-carbazole-9-yl)ethyl]phosphonic acid), Me-4PACz ([4-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphonic acid) and MeO-2PACz ([2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid);

[0012] (2) The thickness of the hole transport layer is 1 nm to 40 nm.

[0013] In some embodiments, the concentration of the alkyl diamine salt in the filling material is 0.1 mg / mL to 2 mg / mL.

[0014] In some embodiments, the filling material further includes a solvent, the alkyl diamine salt is dissolved in the solvent, and the solvent includes DMF (N,N-dimethylformamide).

[0015] In some embodiments, when a filling material is coated on the hole transport layer to form a filling layer, the following steps are included:

[0016] The filling material is coated on the hole transport layer by spin coating, and annealed at 80° C. to 120° C. for 10 min to 30 min, with a spin coating speed of 3000 rpm to 4000 rpm and a spin coating time of 20 s to 30 s.

[0017] In some embodiments, when preparing other structures of the perovskite cell on the filling layer, the following steps are included:

[0018] A perovskite absorption layer, an electron transport layer, a transparent conductive layer and a metal grid electrode are sequentially prepared on the filling layer.

[0019] In some embodiments, the composite layer is an ITO, IZO or IWO intermediate composite layer.

[0020] In some embodiments, the chemical formula of the perovskite light absorbing layer is AB(X n Y 1-n )3, wherein A is a monovalent cation, including but not limited to one or a mixture of several monovalent cations selected from cesium (Cs), rubidium (Rb), methylamine (MA, CH3NH3), and formamidinium (FA, CH2(NH2)2); B is a divalent cation, including but not limited to one or a mixture of several divalent cations selected from lead (Pb), copper (Cu), zinc (Zn), gallium (Ga), tin (Sn), and calcium (Ca); X and Y are monovalent anions, including but not limited to one of iodine (I), bromine (Br), chlorine (Cl), fluorine (F), and thiocyanate ion (SCN); and n is 0 to 1.

[0021] In some embodiments, the laminated battery preparation method satisfies at least one of the following conditions:

[0022] (1) When preparing the perovskite absorption layer, the precursors of each element are mixed in a preset ratio and processed by a solution method such as spin coating, blade coating or slit coating;

[0023] (2) The thickness of the perovskite absorption layer is 0.5 μm to 3 μm.

[0024] In some embodiments, the laminated battery preparation method satisfies at least one of the following conditions:

[0025] (1) The preparation material of the electron transport layer includes C 60 , C 70 And one or more of PCBM;

[0026] (2) The thickness of the electron transport layer is 10 nm to 100 nm.

[0027] In some of the embodiments, the transparent conductive layer is made of one or more of ITO (tin-doped indium oxide), IWO (tungsten-doped indium oxide), IZO (zinc-doped indium oxide) and IZrO (zirconium-doped indium oxide).

[0028] In some embodiments, the metal gate electrode is made of one or more materials selected from Ag, Au and Cu.

[0029] In some of the embodiments, the method for preparing the stacked battery further includes the following steps: preparing a perovskite passivation layer between the perovskite absorption layer and the electron transport layer, and the preparation material of the perovskite passivation layer includes one or more of LiF, MgF2 and propylenediamine hydroiodide.

[0030] In some of the embodiments, the method for preparing the stacked battery further includes the following step: preparing a buffer layer between the electron transport layer and the transparent conductive layer, wherein the thickness of the buffer layer is 4 nm to 30 nm.

[0031] In some of the embodiments, the buffer layer is prepared by using a BCP material through a thermal evaporation process, or is prepared by using a SnO2 material through an atomic layer deposition process (ALD).

[0032] In some of the embodiments, the method for preparing the stacked battery further includes the following step: after preparing the metal grid electrode, preparing an anti-reflection layer, wherein the material for preparing the anti-reflection layer includes one or more of MgF2, LiF and SiO2.

[0033] An embodiment of the present application also provides a stacked battery.

[0034] A stacked battery, the stacked battery comprising a bottom battery and a perovskite battery connected in layers, the hole transport layer of the perovskite battery having a filling layer formed by a filling material, the filling layer at least covering the position on the composite layer not shielded by the hole transport layer, the perovskite layer of the perovskite battery being stacked and connected to the filling layer.

[0035] In some embodiments, the bottom cell includes a crystalline silicon cell or a thin film cell, the crystalline silicon cell includes a PERC cell, a TOPCon cell, a HJT cell or an IBC cell, and the thin film cell includes a GaAs cell, a CdTe cell or a CIGS cell.

[0036] In some embodiments, the stacked battery satisfies at least one of the following conditions:

[0037] (1) The hole transport layer comprises a single layer structure formed by a self-assembled material, or a double layer structure formed by nickel oxide and a self-assembled material, wherein the self-assembled material comprises one or more of 2PACz, Me-4PACz and MeO-2PACz;

[0038] (2) The thickness of the hole transport layer is 1 nm to 40 nm;

[0039] (3) The perovskite cell at least comprises a perovskite absorption layer, an electron transport layer, a transparent conductive layer and a metal grid electrode which are sequentially stacked and connected to the filling layer.

[0040] The above-mentioned method for preparing the stacked battery forms a filling layer by coating a filling material on the hole transport layer of the perovskite battery. The filling layer can fill the position not covered by the hole transport layer, effectively improve the interface contact of the perovskite layer, promote perovskite crystallization, reduce the buried interface defects of the perovskite, increase the voltage and fill factor of the assembled stacked battery, and effectively improve the performance of the photovoltaic module device. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0042] In order to more completely understand the present application and its beneficial effects, the following description will be given in conjunction with the accompanying drawings. In the following description, the same reference numerals represent the same parts.

[0043] Figure 1 A schematic diagram of a method for preparing a stacked battery according to an embodiment of the present invention;

[0044] Figure 2 It is a schematic diagram of the structure of a stacked battery according to an embodiment of the present invention.

[0045] Description of Reference Numerals

[0046] 10. Stacked cell; 100. Bottom cell; 200. Composite layer; 300. Perovskite cell; 310. Hole transport layer; 320. Filling layer; 330. Perovskite absorption layer; 340. Perovskite passivation layer; 350. Electron transport layer; 360. Buffer layer; 370. Transparent conductive layer; 380. Metal grid electrode; 390. Anti-reflection layer. DETAILED DESCRIPTION

[0047] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0048] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0049] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0050] In the present invention, "light-receiving surface or front surface" and "backlight surface or back surface" are only used to distinguish the locations of two opposite surfaces of the battery substrate. In actual working conditions, the "light-receiving surface" is the surface of the battery substrate that mainly receives light, but the "backlight surface" does not necessarily not receive light. In fact, due to the existence of diffusely reflected light, the "backlight surface" can also receive light in actual working conditions.

[0051] In the present invention, unless otherwise indicated, each reaction step may be carried out in the order described herein or may not be carried out in the order described herein. For example, other steps may be included between each reaction step, and the order of the reaction steps may also be appropriately swapped. This can be determined by the skilled person based on conventional knowledge and experience. Preferably, the reaction method herein is carried out sequentially.

[0052] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for a broad range of quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0054] The present application provides a method for preparing a laminated battery to solve the problem that in the process of preparing a laminated battery in the conventional technology, the self-assembled molecular layer and the perovskite layer are in contact at a position on the composite layer of the velvet structure that is not completely covered by the self-assembled molecular layer, resulting in serious carrier recombination and reduced device performance. The method for preparing a laminated battery will be described below in conjunction with the accompanying drawings.

[0055] The method for preparing the laminated battery provided in the embodiments of the present application is exemplary, please refer to Figure 1 As shown, Figure 1 The schematic diagram of the structure of the laminated battery preparation method provided in the embodiment of the present application. The laminated battery preparation method of the present application can be used to prepare the laminated battery 10 to improve the voltage and fill factor of the assembled laminated battery 10 and improve the performance of the photovoltaic module device.

[0056] In order to more clearly illustrate the structure of the laminated battery preparation method, the laminated battery preparation method will be introduced below with reference to the accompanying drawings. Figure 1 As shown, a method for preparing a stacked battery comprises the following steps:

[0057] S1 . Preparing a hole transport layer 310 on the composite layer 200 of the bottom battery 100 .

[0058] S2 . Coating a filling material on the hole transport layer 310 to form a filling layer 320 . The filling layer 320 at least covers a position on the composite layer 200 that is not shielded by the hole transport layer 310 .

[0059] S3. Prepare other structures of the perovskite cell 300 on the filling layer 320 .

[0060] In some embodiments, the bottom cell 100 includes a crystalline silicon cell or a thin film cell.

[0061] In some of the embodiments, the crystalline silicon cell includes but is not limited to a PERC cell (passivated emitter and back contact cell), a TOPCon cell (tunneling oxide passivated contact cell), a HJT cell (crystalline silicon heterojunction solar cell) or an IBC cell (back contact cell), and the thin film cell includes but is not limited to a GaAs cell (gallium arsenide cell), a CdTe cell (cadmium telluride cell) or a CIGS cell (copper indium gallium selenide cell).

[0062] For example, in one specific embodiment, the crystalline silicon cell is a TOPCon cell, and the TOPCon cell structure includes a back electrode, a back anti-reflection layer, a back passivation layer, a P-type doping layer, an N-type silicon substrate, a silicon oxide passivation layer and an N-type polysilicon passivation layer, which are stacked in sequence from bottom to top.

[0063] In some embodiments, the hole transport layer 310 includes a single layer structure formed by a self-assembled material, or nickel oxide (NiO x ) and a double-layer structure formed by a self-assembly material, wherein the self-assembly material includes one or more of 2PACz ([2-(9H-carbazole-9-yl)ethyl]phosphonic acid), Me-4PACz ([4-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphonic acid) and MeO-2PACz ([2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid). It should be noted that nickel oxide (NiO x ) and the double-layer structure formed by the self-assembled material can be nickel oxide (NiO x ) and the self-assembled material form a layer of overlapping structure, in which nickel oxide (NiO x ) forms a main layer, and the self-assembled material forms a sub-layer attached to the main layer, and the main layer and the sub-layer form an overlapping structure.

[0064] In some embodiments, the thickness of the hole transport layer 310 is 1 nm to 40 nm. For example, in one example, the thickness of the hole transport layer 310 includes but is not limited to: 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, or a range between any two of the foregoing.

[0065] In some of these embodiments, the filler material includes an alkyl diamine salt.

[0066] In some embodiments, the number of carbon atoms in the alkyl group of the cation of the alkyl diamine salt is less than 20. The anion includes a halide ion, a sulfonate ion, a formate ion or a tetrafluoroborate ion.

[0067] In some embodiments, the cation of the alkyl diamine salt includes 1,2-ethylenediamine, 1,3-propylenediamine, or 1,4-butylenediamine.

[0068] For example, in one embodiment, the alkyl diamine salt is methylene diamine dihydrochloride (MDAC12).

[0069] In some of the embodiments, the concentration of the alkyl diamine salt in the filling material is 0.1 mg / mL to 2 mg / mL. For example, in one of the examples, the concentration of the alkyl diamine salt in the filling material includes but is not limited to: 0.1 mg / mL, 0.5 mg / mL, 0.8 mg / mL, 1.0 mg / mL, 1.2 mg / mL, 1.5 mg / mL, 1.8 mg / mL, 2.0 mg / mL or a range between any two of the foregoing. The concentration of the alkyl diamine salt in the filling material should not be too large or too small. When the concentration of the alkyl diamine salt is too large, the series resistance increases and the device performance is low; when the concentration of the alkyl diamine salt is too small, the filling effect is poor and there is a more serious interface recombination. Therefore, in this application, the concentration of the alkyl diamine salt of 0.1 mg / mL to 2 mg / mL is most suitable.

[0070] In some embodiments, the filling material further comprises a solvent, and the alkyl diamine salt is dissolved in the solvent.

[0071] In some embodiments, the solvent includes DMF (N,N-dimethylformamide).

[0072] In some embodiments, when the filling material is coated on the hole transport layer 310 to form the filling layer 320, the following steps are included: coating the filling material on the hole transport layer 310 by spin coating, and annealing at a temperature of 80°C to 120°C for 10 min to 30 min. For example, in one example, the annealing temperature includes but is not limited to: 80°C, 90°C, 100°C, 105°C, 110°C, 115°C, 120°C, or a range between any two of the foregoing. The annealing time includes but is not limited to: 10 min, 12 min, 15 min, 18 min, 20 min, 23 min, 25 min, 27 min, 30 min, or a range between any two of the foregoing. The annealing temperature and annealing time should not be too large or too small. When the annealing temperature is too high, the self-assembled monolayer will desorb; when the annealing temperature is too low, the filling effect of the filling material is not ideal.

[0073] In some embodiments, the spin coating speed is 3000 rpm to 4000 rpm, and the spin coating time is 20 s to 30 s. In one example, the spin coating speed includes but is not limited to: 3000 rpm, 3100 rpm, 3200 rpm, 3300 rpm, 3400 rpm, 3500 rpm, 3600 rpm, 3700 rpm, 3800 rpm, 3900 rpm, 4000 rpm or a range between any two of the foregoing. The spin coating time includes but is not limited to: 20 s, 22 s, 23 s, 25 s, 27 s, 29 s, 30 s or a range between any two of the foregoing.

[0074] In some embodiments, when preparing other structures of the perovskite cell 300 on the filling layer 320, the following steps are included: Figure 2 As shown, a perovskite absorption layer 330 , an electron transport layer 350 , a transparent conductive layer 370 and a metal grid electrode 380 are sequentially prepared on the filling layer 320 .

[0075] In some embodiments, the composite layer 200 is an ITO intermediate composite layer.

[0076] In some of the embodiments, the perovskite light absorbing layer is a wide bandgap perovskite light absorbing layer. It can be understood that the wide bandgap is relative to the normal single junction 1.53 eV. The stacked battery 10 needs to adjust the absorption spectrum and current matching, and the bandgap of the top perovskite battery 300 needs to be widened so that photons with weaker energy can pass through the wide bandgap perovskite battery 300 and be absorbed and utilized by the bottom battery 100 below. For example, in some of the examples, the bandgap of the wide bandgap perovskite light absorbing layer is greater than 1.53 eV. For example, the bandgap value specifically includes but is not limited to: 1.55 eV, 1.60 eV, 1.65 eV, 1.68 eV, 1.70 eV or a range between any two of the foregoing.

[0077] In some embodiments, the general chemical formula of the perovskite light absorbing layer is AB(X n Y 1-n )3, wherein A is a monovalent cation, including but not limited to one or a mixture of monovalent cations of cesium (Cs), rubidium (Rb), methylamine (MA, CH3NH3), methylamidine (FA, CH2(NH2)2); B is a divalent cation, including but not limited to one or a mixture of divalent cations of lead (Pb), copper (Cu), zinc (Zn), gallium (Ga), tin (Sn), and calcium (Ca); X and Y are monovalent anions, including but not limited to one of iodine (I), bromine (Br), chlorine (Cl), fluorine (F), and thiocyanate ion (SCN), and n is 0 to 1, preferably, n is 0.2 to 0.25. The value of n includes but is not limited to: 0.1, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range between any two of the foregoing.

[0078] In some embodiments, when preparing the perovskite light absorbing layer, in the preparation of the perovskite precursor solution, the components of the perovskite may specifically be: Cs 0.05 FA 0.8 MA 0.15 Pb(I 0.75 Br 0.25 )3. Cs 0.25 FA 0.75 Pb(I 0.75 Br 0.25 )3. Cs 0.15 FA 0.65 MA 0.2 Pb(I 0.8 Br 0.2 )3 and Cs 0.05 (FA 0.77 MA 0.23 ) 0.95 Pb(I 0.77 Br 0.23)3 or more.

[0079] In some of the embodiments, when preparing the perovskite absorption layer 330, the precursors of each element are mixed according to a preset ratio and then processed by a solution method such as spin coating, blade coating or slit coating.

[0080] In some embodiments, the thickness of the perovskite absorber layer 330 is 0.5 μm to 3 μm. In one example, the thickness of the perovskite absorber layer 330 includes but is not limited to: 0.5 μm, 0.8 μm, 1 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.5 μm, 2.8 μm, 3.0 μm or a range between any two of the foregoing.

[0081] In some embodiments, the preparation material of the electron transport layer 350 includes C 60 , C 70 And one or more of PCBM.

[0082] In some embodiments, the thickness of the electron transport layer 350 is 10 nm to 100 nm. In one example, the thickness of the electron transport layer 350 includes but is not limited to: 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm or a range between any two of the foregoing.

[0083] In some embodiments, the transparent conductive layer 370 is made of one or more materials selected from the group consisting of ITO (tin-doped indium oxide), IWO (tungsten-doped indium oxide), IZO (zinc-doped indium oxide), and IZrO (zirconium-doped indium oxide).

[0084] In some embodiments, the metal gate electrode 380 is made of one or more materials selected from Ag, Au and Cu.

[0085] In some embodiments, the metal gate electrode 380 is prepared by screen printing or deposition process. The thickness of the metal gate electrode 380 can be set according to actual needs, for example, the thickness of the metal gate electrode 380 is 5 nm to 10 nm. In one example, the thickness of the metal gate electrode 380 includes but is not limited to: 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm or a range between any two of the foregoing.

[0086] In some of the embodiments, the method for preparing a stacked battery further includes the following steps: preparing a perovskite passivation layer 340 between the perovskite absorption layer 330 and the electron transport layer 350, and the preparation material of the perovskite passivation layer 340 includes one or more of LiF, MgF2 and propylenediamine hydroiodide.

[0087] In some embodiments, the thickness of the perovskite passivation layer 340 can be set according to actual needs, for example, the thickness of the perovskite passivation layer 340 is 1 nm to 10 nm. In one example, the thickness of the perovskite passivation layer 340 includes but is not limited to: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm or a range between any two of the foregoing.

[0088] In some of the embodiments, the method for preparing a stacked battery further includes the following step: preparing a buffer layer 360 between the electron transport layer 350 and the transparent conductive layer 370 .

[0089] In some of the embodiments, the buffer layer 360 is prepared by using a BCP material through a thermal evaporation process, or is prepared by using a SnO 2 material through an atomic layer deposition process (ALD).

[0090] In some embodiments, the thickness of the buffer layer 360 is 4 nm to 30 nm. In one example, the thickness of the buffer layer 360 includes but is not limited to: 4 nm, 6 nm, 8 nm, 10 nm, 13 nm, 15 nm, 20 nm, 22 nm, 25 nm, 26 nm, 27 nm, 29 nm, 30 nm, or a range between any two of the foregoing.

[0091] In some of the embodiments, the method for preparing a stacked battery further includes the following steps: after preparing the metal grid electrode 380, preparing an anti-reflection layer 390 on the portion of the transparent conductive layer 370 not covered by the metal grid electrode 380, and the preparation material of the anti-reflection layer 390 includes one or more of MgF2, LiF and SiO2.

[0092] In some embodiments, the thickness of the anti-reflection layer 390 can be set according to actual needs. For example, the thickness of the anti-reflection layer 390 is 5 nm to 200 nm. In one example, the thickness of the anti-reflection layer 390 includes but is not limited to: 5 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, or a range between any two of the foregoing.

[0093] An embodiment of the present application further provides a stacked battery 10 .

[0094] A laminated battery 10 is prepared by using the laminated battery preparation method mentioned above.

[0095] An embodiment of the present application further provides a stacked battery 10 .

[0096] A stacked battery 10 includes a bottom battery 100 and a perovskite battery 300 which are stacked and connected. A filling layer 320 formed by a filling material is provided on a hole transport layer 310 of the perovskite battery 300. The filling layer 320 at least covers a position on a composite layer 200 that is not shielded by the hole transport layer 310. A perovskite layer 340 of the perovskite battery 300 is stacked and connected to the filling layer 320.

[0097] In some of the embodiments, the bottom cell of the stacked cell 10 includes a crystalline silicon cell or a thin film cell. The crystalline silicon cell includes a PERC cell, a TOPCon cell, a HJT cell or an IBC cell. The thin film cell includes a GaAs cell, a CdTe cell or a CIGS cell.

[0098] In some of the embodiments, in the stacked battery 10, the hole transport layer 310 includes a single-layer structure formed by a self-assembled material, or a double-layer structure formed by nickel oxide and a self-assembled material, wherein the self-assembled material includes one or more of 2PACz, Me-4PACz and MeO-2PACz.

[0099] In some of the embodiments, the thickness of the hole transport layer of the stacked battery 10 is 1 nm to 40 nm.

[0100] In some of these embodiments, see Figure 2 As shown, the perovskite cell 300 at least includes a perovskite absorption layer 330 , an electron transport layer 350 , a transparent conductive layer 370 and a metal grid electrode 380 which are sequentially stacked and connected to the filling layer 320 .

[0101] In some of these embodiments, see Figure 2 As shown, the perovskite cell 300 further includes one or more of a perovskite passivation layer 340 , a buffer layer 360 , and an anti-reflection layer 390 .

[0102] For example, in one specific example, see Figure 2 As shown, the stacked cell 10 includes the following stacked structure: bottom cell 100, composite layer 200, hole transport layer 310, filling layer 320, perovskite absorption layer 330, perovskite passivation layer 340, electron transport layer 350, buffer layer 360, transparent conductive layer 370, metal grid electrode 380, anti-reflection layer 390. The thickness and material of each film layer in the stacked cell 10 can be selected as described above.

[0103] Example 1

[0104] This embodiment provides a stacked battery 10 .

[0105] The laminated battery 10 of this embodiment is prepared by the following laminated battery preparation method. The laminated battery 10 includes a bottom battery 100 and a perovskite battery 300 connected to each other. Figure 2 As shown, a filling material is provided on the hole transport layer 310 of the perovskite cell 300 to form a filling layer 320, and the filling layer 320 covers the position on the composite layer 200 that is not shielded by the hole transport layer 310. The bottom cell 100 is a HJT cell.

[0106] A method for preparing a laminated battery comprises the following steps:

[0107] S1. Prepare an HJT cell as the bottom cell 100. The HJT cell structure includes a back electrode (including a back anti-reflection layer), a transparent conductive electrode, a P-type microcrystalline silicon, an intrinsic amorphous silicon passivation layer, an N-type silicon substrate, an intrinsic amorphous silicon passivation layer, and an N-type microcrystalline silicon, which are stacked in sequence from bottom to top.

[0108] S2. Prepare an IZO intermediate composite layer 200 on the N-type microcrystalline silicon of the HJT cell.

[0109] S3. A hole transport layer 310 with a single layer structure having a thickness of 2 nm is prepared on the IZO intermediate composite layer 200 by using a self-assembled material, wherein the self-assembled material includes 2PACz ([2-(9H-carbazole-9-yl)ethyl]phosphonic acid).

[0110] S4, coating the filling material on the hole transport layer 310 by spin coating, the spin coating speed is 3000 rpm, the spin coating time is 30 s, and annealing is performed at 100°C for 20 min to form a filling layer 320, and the filling layer 320 covers the position on the composite layer 200 that is not shielded by the hole transport layer 310. The filling material includes solvent DMF and methylenediamine dihydrochloride (MDACl2), and the concentration of methylenediamine dihydrochloride (MDACl2) is 0.5 mg / mL.

[0111] S5, spin-coating the perovskite precursor solution on the filling layer 320 to prepare a perovskite absorption layer 330 with a thickness of 1 μm, and the band gap of the perovskite absorption layer is 1.68 eV. The component of the perovskite in the perovskite precursor solution is Cs 0.05 FA 0.8 MA 0.15 Pb(I 0.75 Br 0.25 )3.

[0112] S6. Prepare a perovskite passivation layer 340 with a thickness of 1 nm using LiF material on the perovskite absorption layer 330.

[0113] S7, on the perovskite passivation layer 340, C 60The material prepares an electron transport layer 350 with a thickness of 12 nm.

[0114] S8. Prepare a buffer layer 360 with a thickness of 10 nm on the electron transport layer 350 using SnO2 as a material by a thermal evaporation process.

[0115] S9. Prepare a transparent conductive layer 370 with a thickness of 40 nm on the buffer layer 360 using an IZO material.

[0116] S10 , preparing a metal gate electrode 380 with a thickness of 100 nm using Ag material on the transparent conductive layer 370 .

[0117] S11, preparing an anti-reflection layer 390 with a thickness of 100 nm using MgF2 material on the metal gate electrode 380.

[0118] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0119] Example 2

[0120] This embodiment provides a stacked battery 10 .

[0121] The structure of the laminated battery 10 of this embodiment is the same as that of the embodiment 1, and the method for preparing the laminated battery is basically the same as that of the embodiment, except that in this embodiment, in step S2, the hole transport layer 310 includes NiO x A bilayer structure with a thickness of 40 nm formed with a self-assembled material, wherein the self-assembled material includes 2PACz ([2-(9H-carbazol-9-yl)ethyl]phosphonic acid).

[0122] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0123] Example 3

[0124] This embodiment provides a stacked battery 10 .

[0125] The structure of the stacked battery 10 of this embodiment is the same as that of embodiment 1, and the method for preparing the stacked battery is basically the same as that of the embodiment, except that in this embodiment, in step S4, the filling material is coated on the hole transport layer 310 by spin coating at a spin coating speed of 4000 rpm and a spin coating time of 20 s.

[0126] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0127] Example 4

[0128] This embodiment provides a stacked battery 10 .

[0129] The structure of the stacked battery 10 of this embodiment is the same as that of embodiment 1, and the method for preparing the stacked battery is basically the same as that of the embodiment, except that in this embodiment, in step S4, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 80° C. for 30 min.

[0130] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0131] Example 5

[0132] This embodiment provides a stacked battery 10 .

[0133] The structure of the stacked battery 10 of this embodiment is the same as that of embodiment 1, and the method for preparing the stacked battery is basically the same as that of the embodiment, except that, in this embodiment, in step S4, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 120° C. for 10 min.

[0134] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0135] Example 6

[0136] This embodiment provides a stacked battery 10 .

[0137] The structure of the stacked battery 10 of this embodiment is the same as that of Example 1, and the method for preparing the stacked battery is basically the same as that of the embodiment, except that, in this embodiment, in step S4, the filling material includes solvent DMF and methylenediamine dihydrochloride (MDACl2), and the concentration of methylenediamine dihydrochloride (MDACl2) is 0.1 mg / mL.

[0138] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0139] Example 7

[0140] This embodiment provides a stacked battery 10 .

[0141] The structure of the stacked battery 10 of this embodiment is the same as that of Embodiment 1, and the method for preparing the stacked battery is basically the same as that of the embodiment, except that, in this embodiment, in step S4, the filling material includes solvent DMF and methylenediamine dihydrochloride (MDACl2), and the concentration of methylenediamine dihydrochloride (MDACl2) is 2 mg / mL.

[0142] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0143] Example 8

[0144] This embodiment provides a stacked battery 10 .

[0145] The structure of the laminated battery 10 of this embodiment is the same as that of the embodiment 1, and the method for preparing the laminated battery is basically the same as that of the embodiment, except that in this embodiment, in step S4, the filling material includes solvent DMF and 2-ethylenediamine formate, and the concentration of 2-ethylenediamine formate is 1 mg / mL.

[0146] Comparative Example 1

[0147] This comparative example provides a stacked battery 10 .

[0148] The structure of the stacked battery 10 of this comparative example is basically the same as that of Example 1, and the method for preparing the stacked battery is basically the same as that of the example, except that in this comparative example, step S4 is omitted, and in step S5, the perovskite absorption layer 330 is directly prepared on the hole transport layer 310 of step S3.

[0149] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0150] Comparative Example 2

[0151] This comparative example provides a stacked battery 10 .

[0152] The structure of the stacked battery 10 of this comparative example is basically the same as that of Example 1, and the method for preparing the stacked battery is basically the same as that of the example, except that in this comparative example, in step S4, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 70° C. for 40 min.

[0153] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0154] Comparative Example 3

[0155] This comparative example provides a stacked battery 10 .

[0156] The structure of the stacked battery 10 of this comparative example is basically the same as that of Example 1, and the method for preparing the stacked battery is basically the same as that of the example, except that in this comparative example, in step S4, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 130° C. for 5 min.

[0157] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0158] Comparative Example 4

[0159] This comparative example provides a stacked battery 10 .

[0160] The structure of the laminated battery 10 of this comparative example is basically the same as that of Example 1, and the method for preparing the laminated battery is basically the same as that of the example, except that in this comparative example, in step S4, the filling material includes solvent DMF and methylenediamine dihydrochloride (MDACl2), and the concentration of methylenediamine dihydrochloride (MDACl2) is 0.05 mg / mL.

[0161] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0162] Comparative Example 5

[0163] This comparative example provides a stacked battery 10 .

[0164] The structure of the laminated battery 10 of this comparative example is the same as that of Example 1, and the method for preparing the laminated battery is basically the same as that of the example, except that in this comparative example, in step S4, the filling material includes solvent DMF and methylenediamine dihydrochloride (MDACl2), and the concentration of methylenediamine dihydrochloride (MDACl2) is 3 mg / mL.

[0165] The prepared stacked battery 10 was subjected to performance tests, and the test data included energy conversion efficiency (%), open circuit voltage (V), short circuit current density (mA / cm 2 ) and filling factor (%), the test results are shown in Table 1.

[0166] Table 1

[0167]

[0168] As can be seen from Table 1, in Examples 1 to 8, the filling material is respectively coated on the hole transport layer 310 by spin coating to form a filling layer 320. The filling layer 320 can fill the partially uncovered position of the hole transport layer 310, effectively improving the interface contact of the perovskite layer, promoting the crystallization of perovskite, and reducing the interface defects of the perovskite buried bottom. In Comparative Example 1, the filling layer 320 is missing, and the position on the composite layer 200 of the velvet structure of the bottom battery 100 of the stacked battery 10 in Comparative Example 1 that is not completely covered by the self-assembled molecular layer will cause the composite layer and the perovskite layer to contact, resulting in carrier recombination, which reduces the device performance, manifested as low energy conversion efficiency, low open circuit voltage, low short-circuit current density, and small filling factor, etc. Therefore, the energy conversion efficiency (%), open circuit voltage (V), short-circuit current density (mA / cm 2 ) and filling factor (%) are higher than those of Comparative Example 1.

[0169] By comparing Example 1 with Comparative Example 2, it can be seen that in step S4 of Comparative Example 2, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 70°C for 40 min. When preparing the filling layer 320 in Comparative Example 2, the annealing temperature is too low, resulting in poor formation effect of the filling layer 320. The filling layer 320 cannot be completely filled in the position on the composite layer 200 of the velvet structure of the bottom battery 100 that is not completely covered by the self-assembled molecular layer, which will cause the composite layer to contact the perovskite layer, resulting in carrier recombination, which reduces the device performance, manifested in low energy conversion efficiency, low open circuit voltage, low short-circuit current density, and small filling factor, etc.

[0170] Similarly, by comparing Example 1 with Comparative Example 3, it can be seen that in step S4 of Comparative Example 3, after the filling material is coated on the hole transport layer 310 by spin coating, it is annealed at 130°C for 5 min. When preparing the filling layer 320 in Comparative Example 3, the annealing temperature is too high, resulting in desorption of the self-assembled monolayer, resulting in carrier recombination, and reducing the device performance, which is manifested as low energy conversion efficiency, low open circuit voltage, low short circuit current density, and small filling factor, etc. In addition, if the annealing temperature is too high, it will also cause energy waste, and has high requirements for production equipment, and the production cost is too high.

[0171] By comparing Example 1 with Comparative Example 4, it can be seen that in step S4 of Comparative Example 4, the concentration of methylenediamine dihydrochloride (MDACl2) is 0.05 mg / mL. When preparing the filling layer 320 in Comparative Example 4, the concentration of the effective ingredient of the filling material is too low, resulting in poor formation of the filling layer 320, or the filling layer 320 cannot be formed at some positions. The filling layer 320 cannot be completely filled in the positions on the composite layer 200 of the velvet structure of the bottom battery 100 that are not completely covered by the self-assembled molecular layer, and the composite layer and the perovskite layer are in contact, resulting in carrier recombination, which reduces the device performance, manifested as low energy conversion efficiency, low open circuit voltage, low short-circuit current density, and small filling factor, etc.

[0172] By comparing Example 1 with Comparative Example 5, it can be seen that in step S4 of Comparative Example 5, the concentration of methylenediamine dihydrochloride (MDACl2) is 3 mg / mL. When preparing the filling layer 320 in Comparative Example 5, the concentration of the effective component of the filling material is too high, which increases the series resistance and affects the performance of the hole transport layer 310, which is manifested as low energy conversion efficiency, low open circuit voltage, low short circuit current density, and small filling factor, etc. In addition, if the concentration of methylenediamine dihydrochloride (MDACl2) is too high, it will also cause an increase in material costs and excessively high production costs.

[0173] In summary, the method for preparing a stacked battery of the present application forms a filling layer 320 by coating a filling material on the hole transport layer 310 of the perovskite battery 300. The filling layer 320 can fill the partially uncovered position of the hole transport layer 310, effectively improving the interface contact of the perovskite layer, promoting perovskite crystallization, reducing the buried interface defects of the perovskite, and increasing the voltage and fill factor of the assembled stacked battery 10, thereby effectively improving the performance of the photovoltaic module device.

[0174] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0175] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0176] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a laminated battery, It is characterized in that The steps include: preparing a hole transport layer on the composite layer of the bottom cell; Coating a filling material on the hole transport layer to form a filling layer, wherein the filling layer at least covers a position on the composite layer that is not shielded by the hole transport layer; the filling material comprises an alkyl diamine salt, wherein the number of carbon atoms of the alkyl group in the cation of the alkyl diamine salt is less than 20, and the anion comprises a halogen ion, a sulfonate ion, a formate ion or a tetrafluoroborate ion; and Other structures of the perovskite cell are prepared on the filling layer.

2. The method for preparing a laminated battery according to claim 1, It is characterized in that The stacked battery preparation method meets at least one of the following conditions: (1) The concentration of the alkyl diamine salt in the filling material is 0.1 mg / mL to 2 mg / mL; (2) The filling material further includes a solvent, the alkyl diamine salt is dissolved in the solvent, and the solvent includes DMF; (3) When a filling material is coated on the hole transport layer to form a filling layer, the method comprises the following steps: The filling material is coated on the hole transport layer by spin coating, and annealed at 80° C. to 120° C. for 10 min to 30 min, with a spin coating speed of 3000 rpm to 4000 rpm and a spin coating time of 20 s to 30 s.

3. The method for preparing a laminated battery according to any one of claims 1 to 2, It is characterized in that When preparing other structures of the perovskite battery on the filling layer, the following steps are included: A perovskite absorption layer, an electron transport layer, a transparent conductive layer and a metal grid electrode are sequentially prepared on the filling layer.

4. The method for preparing a laminated battery according to claim 3, It is characterized in that The stacked battery preparation method meets at least one of the following conditions: (1) The composite layer is an ITO, IZO or IWO intermediate composite layer; (2) The general chemical formula of the perovskite light-absorbing layer is AB(X n Y 1-n ) 3 , wherein A is a monovalent cation, including one or a mixture of several monovalent cations selected from cesium, rubidium, methylamine, and methylamidine; B is a divalent cation, including one or a mixture of several divalent cations selected from lead, copper, zinc, gallium, tin, and calcium; X and Y are monovalent anions, including one of iodine, bromine, chlorine, fluorine, and thiocyanate ions, and n is 0 to 1; (3) When preparing the perovskite absorption layer, the precursors of each element are mixed in a preset ratio and then processed by a solution method such as spin coating, blade coating or slit coating; (4) The thickness of the perovskite absorption layer is 0.5 μm to 3 μm; (5) The preparation material of the electron transport layer includes C 60 , C 70 And one or more of PCBM; (6) The thickness of the electron transport layer is 10 nm to 100 nm; (7) The transparent conductive layer is made of one or more materials selected from the group consisting of ITO, IWO, IZO and IZrO; (8) The metal gate electrode is made of one or more materials selected from Ag, Au and Cu.

5. The method for preparing a laminated battery according to claim 3, It is characterized in that The stacked battery preparation method further comprises the following steps: preparing a perovskite passivation layer between the perovskite absorption layer and the electron transport layer, wherein the preparation material of the perovskite passivation layer comprises LiF, MgF 2 and one or more of propylenediamine hydroiodide.

6. The method for preparing a laminated battery according to claim 3, It is characterized in that The stacked battery preparation method further includes the following steps: preparing a buffer layer between the electron transport layer and the transparent conductive layer, wherein the thickness of the buffer layer is 4 nm to 30 nm.

7. The method for preparing a laminated battery according to claim 3, It is characterized in that The stacked cell preparation method further comprises the following steps: after preparing the metal grid electrode, preparing an anti-reflection layer, wherein the preparation material of the anti-reflection layer comprises MgF 2 , LiF and SiO 2 One or more of .

8. A laminated battery, It is characterized in that The stacked battery includes a bottom battery and a perovskite battery connected in layers. The hole transport layer of the perovskite battery has a filling layer formed by a filling material, and the filling layer at least covers the position on the composite layer that is not shielded by the hole transport layer. The perovskite layer of the perovskite battery is stacked and connected to the filling layer.

9. The laminated battery according to claim 8, It is characterized in that The bottom cell includes a crystalline silicon cell or a thin film cell, the crystalline silicon cell includes a PERC cell, a TOPCon cell, a HJT cell or an IBC cell, and the thin film cell includes a GaAs cell, a CdTe cell or a CIGS cell.

10. The laminated battery according to claim 8 or 9, It is characterized in that The stacked battery satisfies at least one of the following conditions: (1) The hole transport layer comprises a single layer structure formed by a self-assembled material, or a double layer structure formed by nickel oxide and a self-assembled material, wherein the self-assembled material comprises one or more of 2PACz, Me-4PACz and MeO-2PACz; (2) The thickness of the hole transport layer is 1 nm to 40 nm; (3) The perovskite cell at least comprises a perovskite absorption layer, an electron transport layer, a transparent conductive layer and a metal grid electrode which are sequentially stacked and connected to the filling layer.

Citation Information

Cited By

  • Preparation method of efficient and stable perovskite solar cell combining ionic compound interface modification and polymer material external packaging

    CN119546047A