Geopolymer compositions and methods of making same

By carbonating the slag powder and combining it with volcanic ash materials and alkali sources, the problems of short service life and high environmental load of geopolymers are solved, and an environmentally friendly geopolymer material that maintains strength during the pouring process is achieved.

CN118871402APending Publication Date: 2024-10-29TOKUYAMA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027726.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-04-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing geopolymers can be used for a short time during the pouring process, and high-temperature treatment results in reduced strength and high environmental load, making it difficult to meet the acid resistance, heat resistance, and CO2 suppression requirements of materials such as concrete.

Method used

By carbonating slag powder, carbonated slag powder containing CO2 and bound water is generated, and combined with volcanic ash materials and alkali sources to extend the usable time of geopolymers and reduce environmental load at the same time.

Benefits of technology

While maintaining strength performance, it greatly extends the usable time of geopolymers. It is suitable as a cement substitute material for concrete, etc. It has acid resistance, heat resistance, CO2 inhibition performance, and low environmental load.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118871402A_ABST
    Figure CN118871402A_ABST
Patent Text Reader

Abstract

Provided is a powdered geopolymer composition containing: an active filler comprising a carbonated slag micropowder and a pozzolanic material powder; and a powdered alkali source comprising at least one selected from the group consisting of alkali metal silicate powder and alkali metal carbonate powder, and the carbonated slag fine powder contains 0.1-2.0 mass% of CO2 and 0.26-1.0 mass% of bound water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a slow setting technology of geopolymer. Background Art

[0002] Geopolymer is defined as "a material that is hardened using a raw material (active filler) mainly composed of amorphous aluminum silicate and an aqueous solution (alkali source) of alkali metal silicates, carbonates, and hydroxides instead of cement clinker." It is an inorganic material that is expected to be used as a construction material because it can achieve acid resistance, heat resistance, CO2 suppression, and large-scale use of industrial by-products compared to cement hardening.

[0003] In recent years, in order to improve the strength performance and material transfer resistance at room temperature, which are the weaknesses of geopolymers using only fly ash as active fillers, slag powder has been used in combination with fly ash as an active filler. However, by using slag powder as an active filler, the usable time (setting time) of the geopolymer is shortened to about 15 to 40 minutes, which is a major disadvantage that sufficient time cannot be ensured in the pouring operation.

[0004] Therefore, in order to extend the usable time (setting time) of geopolymer, the following method is disclosed in Patent Document 1: slag powder is heated at 200-1000°C, thereby obtaining a slow-setting active filler for geopolymer, and the geopolymer solidified body is obtained by using the active filler. Although the usable time can be extended by the method shown in Patent Document 1, a significant reduction in bending strength will occur due to heating at 800°C. It is believed that this is because heating causes the slag crystal structure to change, and the glass phase in the slag powder, which is a reactant of the geopolymer reaction, is converted into a crystalline state (calcium feldspar and mavinite) that is inactive in the reaction. Furthermore, it is believed that due to the reduction in the total amount of reactants (glass phase) in the active filler, the strength will also decrease in the long term. Furthermore, the slag powder needs to be sintered at high temperature, so huge thermal energy is required, and it can be expected that CO2 discharge caused by thermal energy will have a large environmental load.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-031370 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] Geopolymer compositions are often used as cement substitutes as binders for concrete and mortar. On the other hand, in the case of pouring cement concrete, concrete is mixed in a factory, transported by a truck mixer, and poured on site using a concrete pump truck. The Civil Engineering Society and the Architectural Society set a standard of 120 minutes or less for the allowable time from mixing concrete to the end of pouring when the outside air temperature is below 25°C and 90 minutes or less for exceeding 25°C. Therefore, in order to generalize geopolymer concrete, a geopolymer composition that maintains the same fresh properties as cement concrete after 120 minutes after mixing is sought.

[0010] The present invention has been made based on the above circumstances, and an object of the present invention is to provide a geopolymer composition and a method for producing the same which can significantly extend the usable time while maintaining strength and has a low environmental load.

[0011] Solutions for solving problems

[0012] The inventors of the present invention have conducted repeated and in-depth studies to obtain a geopolymer composition that can significantly extend the usable time while maintaining strength and has a low environmental load. As a result, it was found that the effect of extending the usable time (setting time) of the geopolymer can be obtained by carbonating the slag fine powder. It was also found that the bound water of the slag fine powder generated by the carbonation treatment of the slag fine powder contributes to the extension of the usable time.

[0013] That is, according to the present invention, there are provided a geopolymer composition which can significantly extend the usable time while maintaining strength and has a low environmental load, and a method for producing the same.

[0014] In other words, the first invention is a geopolymer composition comprising: an active filler comprising carbonated slag powder and pozzolanic material and an alkali source,

[0015] The carbonated slag powder contains 0.1 mass % to 2.0 mass % of CO 2 and 0.26 mass % to 1.0 mass % of bound water.

[0016] The carbonated slag fine powder preferably contains 1.0 mass % to 2.0 mass % of CO 2 and 0.5 mass % to 1.0 mass % of bound water.

[0017] More preferably, the carbonated slag fine powder contains 1.5% by mass to 2.0% by mass of CO 2 and 0.75% by mass to 1.0% by mass of bound water.

[0018] The carbonated slag powder is preferably obtained by carbonation treatment under wet conditions in which 0.5 parts by mass or more of water is present relative to 1 part by mass of the slag powder.

[0019] The second present invention is a powdered geopolymer composition, characterized in that the alkali source contained in the geopolymer composition is in powder form and includes at least one selected from alkali metal silicate powder and alkali metal carbonate powder.

[0020] The alkali source is preferably an alkali metal silicate powder or an alkali metal carbonate powder.

[0021] The alkali metal silicate powder is preferably sodium silicate powder. In addition, the alkali metal carbonate powder is preferably sodium carbonate powder.

[0022] The third present invention is a geopolymer composition comprising the aforementioned powdered geopolymer composition and water.

[0023] The fourth present invention is a method for producing a geopolymer composition, which comprises mixing the aforementioned powdered geopolymer composition with water.

[0024] The fifth present invention is a geopolymer hardened body, which is a hardened body of the aforementioned geopolymer composition.

[0025] Effects of the Invention

[0026] By using carbonated slag powder containing bound water as an active filler for geopolymer, a geopolymer composition can be obtained which can achieve a significant extension of the usable time (setting time) while maintaining strength, and has a low environmental load. Therefore, it can be used as a cement substitute for concrete and other binding materials, and can be used universally and appropriately in the construction industry for the purposes of acid resistance, heat resistance, CO2 suppression, and large-scale use of industrial by-products. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a simplified diagram of an apparatus for carbonation treatment of slag micropowder slurry.

[0028] Figure 2 It is a schematic diagram of an apparatus for evaporation and drying of carbonated slag powder slurry. DETAILED DESCRIPTION

[0029] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to the embodiment. It should be noted that "part" and "%" in the present specification are based on mass unless otherwise specified.

[0030] (Geoporm Composition)

[0031] The geopolymer composition of the present invention contains: an active filler including carbonated slag powder and volcanic ash material, an alkali source and water, wherein the carbonated slag powder contains 0.1 mass % to 2.0 mass % of CO2 and 0.26 mass % to 1.0 mass % of bound water.

[0032] (Active filler)

[0033] In the present invention, the active filler comprises carbonated slag powder and volcanic ash material. The active filler comprises carbonated slag powder and volcanic ash material as main components, and the total content of carbonated slag powder and volcanic ash material in the active filler as a whole is preferably 90 mass % or more, more preferably 95 mass % or more, and particularly preferably substantially 100 mass %.

[0034] (Carbonated slag powder)

[0035] Carbonated slag powder contained in the active filler is manufactured by carbonating slag powder, and it comprises CO more than 0.1 mass % and below 2.0 mass % , and comprise bound water more than 0.26 mass % and below 1.0 mass %.CO and bound water, if not satisfying the scope simultaneously, then can't significantly extend the usable time.In order to further extend the usable time, the carbonated slag powder preferably comprises CO more than 1.0 mass % and below 2.0 mass % , and comprise bound water more than 0.5 mass % and below 1.0 mass %, and then, in order to ensure the usable time of the geopolymer composition of the operation time within 120 minutes of the irrigation operation on the spot with truck agitator transportation, the carbonated slag powder preferably comprises CO more than 1.5 mass % and below 2.0 mass %, and comprise bound water more than 0.75 mass % and below 1.0 mass %.

[0036] The slag powder that becomes the raw material of carbonation slag powder is to generate cast iron while producing, and it comprises CaO, SiO , Al O , MgO as main component.In addition, the kind of slag is not particularly limited, and can be any one in blast furnace slag, steelmaking slag, but preferred blast furnace water quenching slag powder from the viewpoint of reactivity, from the viewpoint of intensity embodiment of the geopolymer hardened body obtained by using the carbonation slag powder manufactured by carbonation treatment, preferably use JIS A6206 regulation, do not add gypsum and sulfur trioxide is below 3 mass % and ignition loss is below 3 mass % blast furnace water quenching slag powder as raw material.

[0037] (Method for producing carbonation slag powder)

[0038] For the carbonation method of slag powder, there are known methods: a method of carbonation in a gas containing a wet component; a method of blowing CO2 gas into the slag powder while the slag powder is immersed in water, etc. In the method in the gas, carbonation takes a considerable time, so it is impossible to expect productivity at an industrial level. In addition, carbonated slag powder containing sufficient bound water cannot be obtained. Therefore, it becomes important to carry out the process under wet conditions such as a slurry state or a state immersed in water. In the wet method, carbonated slag powder can be obtained in about a few hours, and carbonated slag powder containing sufficient bound water can be reliably obtained. In the case of the wet method, regarding the mixing ratio of slag powder and water, water is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and further preferably 0.9 parts by mass or more relative to 1 part by mass of slag powder.

[0039] (Volcanic ash material)

[0040] The volcanic ash material is a material having volcanic ash activity, and specific examples thereof include coal ash, biomass ash, fumed silica, volcanic ash, and metakaolinite. In the present invention, fly ash such as coal ash and biomass ash is preferred, and fly ash for concrete is particularly preferred.

[0041] Fly ash is fine ash recovered from exhaust gas by a vacuum cleaner from coal ash and other by-products in coal-fired power plants, etc., and is a substance with volcanic ash activity and SiO2 and Al2O3 as main components. In JIS A 6201, based on particle size and flow rate value, the substances specified in types I to IV are preferred. The standard of fly ash is not particularly limited, and types I and II with fine particle size and high reactivity are more preferred. In addition, other types of ashes can also be used in combination.

[0042] The content of the volcanic ash material in the active filler relative to the total mass of the volcanic ash material and the carbonated slag powder is preferably 50 to 90% by mass, more preferably 60 to 85% by mass. When the content is 50% by mass or more, it is also preferred from the viewpoint of being able to maintain good fluidity, easily obtain sufficient workability, and effectively utilize and expand the volcanic ash material when mixed with water to form a geopolymer composition. In addition, when the content is 90% by mass or less, good strength of the geopolymer composition hardened body can be obtained at the initial age.

[0043] (Alkali source)

[0044] The alkali source can be any of an alkali metal salt or an alkaline earth metal salt. From the viewpoint of the durability of the geopolymer hardened body, it is preferred to use a salt of an alkali metal element. In addition, the salt can also be a silicate, a hydroxide, or a carbonate, and its state is any of a liquid or a powder, and can be an anhydrous substance, a hydrate, or an aqueous solution of the salt. As an alkali source, from the viewpoint of cost and strength embodiment, it is more preferred to include an alkali metal silicate. By mixing and using an alkali metal silicate with other salts such as an alkali metal carbonate, the physical properties of the geopolymer composition can be arbitrarily adjusted. As an alkali metal silicate, sodium silicate (SiO2 / NaO2 molar ratio: about 1.95 to 3.4), sodium metasilicate (1 kind, 2 kinds), potassium silicate, potassium metasilicate, lithium silicate, etc. can be cited.

[0045] When the geopolymer composition contains an alkali metal silicate, the molar ratio Si / AL of silicon (Si) contained in the alkali metal silicate to the alkali metal element (AL) contained in the alkali source is preferably 0.05 to 0.85. By making Si / AL 0.05 or more, the shrinkage of the hardened geopolymer composition can be reduced, and by making Si / AL 0.85 or less, the fluidity that makes it easy to use the geopolymer composition for field work can be ensured. In view of the above, Si / AL is more preferably 0.2 to 0.75.

[0046] The molar ratio AL / W of the alkali metal element (AL) contained in the alkali source of the geopolymer composition to water (W) is preferably 0.05 to 0.3. By making AL / W 0.05 or more, the compressive strength of the hardened geopolymer composition can be ensured at room temperature, and by making AL / W 0.3 or less, the fluidity of the geopolymer composition can be ensured to facilitate the use of the geopolymer composition in field operations. From the above viewpoints, AL / W is more preferably 0.05 to 0.18, and further preferably 0.08 to 0.12.

[0047] In addition to the above, various admixtures and admixtures can be added to the geopolymer composition of the present invention within the range that does not impair the effects of the present invention. For example, known materials used in concrete such as flow agents, shrinkage reducers, rust inhibitors, waterproofing materials, retarders, defoamers, dust reducing agents, pigments, and calcium carbonate powders can be cited.

[0048] In addition to the above, various aggregates can be further added to the geopolymer composition of the present invention according to the use of the geopolymer composition. For example, known aggregates used in concrete such as lightweight aggregates, ordinary aggregates, heavy aggregates, limestone aggregates, slag aggregates, and silica sand can be cited.

[0049] (Method for producing geopolymer composition)

[0050] The geopolymer composition of the present invention can be produced by mixing the active filler including the carbonated slag powder and the volcanic ash material, the alkali source, and water, and various mixed materials and aggregates as required, simultaneously or sequentially in a predetermined amount, and kneading them in a suitable kneading device. The kneading device is not particularly limited, and examples thereof include a forced twin-screw kneader for kneading concrete.

[0051] Regarding the method for manufacturing the geopolymer composition, for example, when the alkali source is in powder form, the method includes the following steps: a powder mixing step, in which active fillers, powdered alkali sources and aggregates are mixed in powder form; and a kneading step, in which water is added for kneading after the powder mixing step. When the alkali source is not in powder form, the method includes the following steps: a powder mixing step, in which active fillers and aggregates are mixed in powder form; and a kneading step, in which an aqueous solution of the alkali source is added for kneading after the powder mixing step. It should be noted that a secondary kneading step may be provided after the kneading step to mix and knead admixtures such as flow agents and retarders.

[0052] (Powdered geopolymer composition)

[0053] The powdered geopolymer composition of the present invention contains: an active filler comprising carbonated slag powder and volcanic ash material powder; and a powdered alkali source comprising at least one selected from alkali metal silicate powder and alkali metal carbonate powder.

[0054] (Active filler)

[0055] The active filler of the powdered geopolymer composition of the present invention is the active filler used in the above-mentioned geopolymer composition, which mainly contains carbonated slag powder and volcanic ash material powder.

[0056] (Powdered alkali source)

[0057] The powdered alkali source of the powdered geopolymer composition of the present invention comprises at least one selected from alkali metal silicate powder and alkali metal carbonate powder.

[0058] (Alkali metal silicate powder)

[0059] As the alkali metal silicate powder, there can be mentioned sodium silicate powder (SiO2 / NaO2 molar ratio: about 1.95 to 3.4), sodium metasilicate powder (one type, two types), potassium silicate powder, potassium metasilicate powder, lithium silicate powder, etc. In terms of excellent strength, durability, and being a relatively cheap powder material, sodium silicate powder (SiO2 / NaO2 molar ratio: about 1.950 to 2.2, H2O=about 20 mass%) is preferred.

[0060] (Alkali Metal Carbonate Powder)

[0061] Examples of the alkali metal carbonate powder include sodium carbonate (Na2CO3), potassium carbonate (K2CO3), lithium carbonate (Li2CO3), etc. Sodium carbonate powder is preferred because it is inexpensive and highly reactive with slag fine powder.

[0062] The powdered alkali source may contain at least one selected from alkali metal silicate powder and alkali metal carbonate powder, and preferably consists of alkali metal silicate powder and alkali metal carbonate powder from the viewpoint of developing strength.

[0063] When the powdered geopolymer composition contains alkali metal silicate powder and alkali metal carbonate powder, the molar ratio Si / AL of silicon (Si) contained in the powdered alkali source, alkali metal silicate powder and alkali metal carbonate powder to alkali metal element (AL) is preferably 0.05 to 0.85. By making Si / AL 0.05 or more, the shrinkage of the hardened geopolymer composition can be reduced, and by making Si / AL 0.85 or less, the fluidity of the geopolymer composition can be ensured to facilitate the use of the geopolymer composition in field operations. In view of the above, Si / AL is more preferably 0.2 to 0.75.

[0064] (Method for producing powdered geopolymer composition)

[0065] The preparation of the powdered geopolymer composition of the present invention includes the following powder mixing step: mixing the carbonated slag powder and volcanic ash material powder as active fillers with at least one selected from alkali metal silicate powder and alkali metal carbonate powder as powdered alkali source in the form of powder. It should be noted that after the powder mixing step, a secondary powder mixing step of mixing various mixed materials such as powdered flow agent, retarder, and aggregate can be provided.

[0066] The powdered geopolymer composition of the present invention can be used in the form of a premixed composition. By making a premixed composition, the geopolymer composition of the present invention can be manufactured simply by mixing the premixed composition with water. Specifically, it contains: an active filler including carbonated slag powder and volcanic ash material powder, a powdered alkali source including at least one selected from alkali metal silicate powder and alkali metal carbonate powder, and water. In addition, the powdered geopolymer composition and geopolymer composition of the present invention may also exist as part of the constituent raw materials when making mortar, concrete, etc.

[0067] In addition to the above, various powdered admixtures and admixtures may be added to the powdered geopolymer composition of the present invention within the range that does not impair the effects of the present invention. Examples thereof include known materials used in concrete such as flow agents, shrinkage reducers, rust inhibitors, waterproofing materials, retarders, defoamers, dust reducing agents, pigments, and calcium carbonate powder.

[0068] In addition to the above, various aggregates can be further added to the powdered geopolymer composition of the present invention according to the use of the geopolymer composition. For example, known aggregates used in concrete such as lightweight aggregates, ordinary aggregates, heavy aggregates, limestone aggregates, slag aggregates, and silica sand can be cited.

[0069] (Method for producing geopolymer composition using powdered geopolymer composition)

[0070] The geopolymer composition of the present invention can be produced by mixing the powdered geopolymer composition, water, and various mixed materials and aggregates as required simultaneously or sequentially in a predetermined amount, and kneading them in a suitable kneading device. The kneading device is not particularly limited, and examples thereof include a forced twin-screw kneading machine for kneading concrete.

[0071] The method for producing a geopolymer composition includes, for example, the following steps: a powder mixing step, in which the powdered geopolymer composition of the present invention is mixed with aggregates; and a kneading step, in which water is added for kneading after the powder mixing step. It should be noted that a second kneading step may be provided after the kneading step, in which a flow agent, a retarder, or other admixture is mixed with the admixture for kneading.

[0072] (Method for producing a hardened body of a geopolymer composition)

[0073] After the mixing step or the secondary mixing step of the geopolymer composition, the geopolymer composition is cured at a temperature range of 5°C to 90°C, thereby obtaining a geopolymer hardened body as a hardened product of the geopolymer composition. In particular, when an alkali metal silicate and an alkali metal carbonate are used in combination as the alkali source of the geopolymer composition, a geopolymer hardened body having excellent compressive strength can be obtained by curing at a room temperature of 5 to 35°C. Other curing conditions are not particularly limited, and may be generally used curing conditions. For example, steam curing, sealed curing, curing in gas, curing in water, etc. may be used.

[0074] Compared with the known geopolymer composition using the existing slag powder, the geopolymer composition can extend the service life to more than 120 minutes while maintaining the strength, so it is excellent in construction and workability. Therefore, the geopolymer composition of the present invention can be mixed in the same way as the cement concrete as a general material in the factory, transported with a truck mixer, and poured on site based on a concrete pump truck, etc. In addition, when the slag powder is carbonated, carbonates can be formed on the slag particle surface with calcium, magnesium, etc. Thus, there is the advantage of being able to realize the fixation and effective utilization of CO2 as a greenhouse effect gas. In addition, the CO2 gas used in the carbonic acid gas can include a certain amount of CO2 such as industrial waste gas. Therefore, the geopolymer hardened body obtained using the geopolymer composition of the present invention has a low environmental load compared with the existing geopolymer composition, and can replace cement composition in various applications as a binding material for concrete.

[0075] Example

[0076] The present invention is further described in detail by listing specific embodiments below. However, the present invention is not limited to the following embodiments. Various modifications and application examples are also included in the present invention without significantly impairing the advantages of the present invention.

[0077] (raw materials)

[0078] Active fillers

[0079] (1) Fly ash (FA): Fly ash type II (based on JIS A 6201)

[0080] (2) Blast furnace slag powder (BFS): Blast furnace slag powder 4000 (according to JIS A 6206)

[0081] Powdered alkali source (alkali metal silicate powder, alkali metal carbonate powder)

[0082] (3) Powdered sodium silicate: Sodium silicate powder (SiO2 / Na2O molar ratio = 1.98, H2O = about 20% by mass, manufactured by our company)

[0083] (4) Soda ash: Sodium carbonate powder (produced by our company)

[0084] Other raw materials

[0085] (5) Aggregate: Fine aggregate (JIS standard sand)

[0086] (6) Water: Ion exchange water

[0087] (7) Ordinary cement: Ordinary Portland cement (according to JIS R 5210)

[0088] [Carbonation treatment of slag powder]

[0089] The apparatus for carrying out the carbonation treatment of slag fine powder is shown in Figure 1 .

[0090] like Figure 1 As shown, 1000 g of slag powder slurry (6) (slag powder: purified water = mass ratio 1:1) is added to a 2000 mL polycarbonate gas cleaning bottle (4), and a prescribed flow of CO2 gas is blown into the gas cleaning bottle (4) from a CO2 gas storage bottle (1) through a nozzle (2). The gas cleaning bottle (4) is maintained at a prescribed temperature using a constant temperature water tank (3), and then stirred at 300 min by a stirrer (7). -1 (rpm) while stirring the gas cleaning bottle (4), a carbonation treatment is carried out for a predetermined time to obtain a carbonated slag powder slurry. Figure 2 As shown, a carbonation slag powder slurry (10) is added into a heat-resistant container (9), and the purified water contained in the carbonation slag powder slurry (10) is evaporated to dryness in a dryer (8). It should be noted that the amount of CO2 and the amount of bound water can be controlled by the flow rate of carbonic acid gas, the treatment temperature, the mass ratio of slag powder to purified water, the stirring speed, etc. The carbonation treatment conditions of the carbonation slag powders BFS-A and BFS-B are recorded in the following Table 1.

[0091] [Heat treatment of slag powder]

[0092] For the slag powder, an electric furnace was used, and the BFS-400 was kept at 400°C for 3 hours, the BFS-700 was kept at 700°C for 3 hours, and the BFS-800 was kept at 800°C for 3 hours. After heating, it was transferred outside the furnace for air cooling. It should be noted that the heating rate from room temperature to each heating temperature was 20°C / min.

[0093] [Quantitative method for CO2 amount and bound water amount]

[0094] The dried carbonated slag powder was analyzed by a thermogravimetric differential thermal analyzer at a temperature increase rate of 20°C / min from room temperature to 1000°C in a N2 atmosphere.

[0095] The mass reduction from room temperature to 500°C was recorded as the amount of bound water, and the amount of hydrate contained in the carbonated slag powder was also calculated when the hydration product was assumed to be a calcite-based hydrate (2CaO·Al2O3·SiO2·8H2O, molecular weight 418.3).

[0096] In addition, it is estimated that the mass reduction from 500° C. to 700° C. is derived from CO 2 released by thermal decomposition of calcium carbonate, and the amount of CO 2 and the amount of calcium carbonate (molecular weight 100.1) are calculated from the mass reduction from 500° C. to 700° C. These results are shown in Table 1.

[0097] [Physical properties of carbonated slag powder]

[0098] Table 1 below shows the physical properties of the carbonated slag powder.

[0099] [Table 1]

[0100]

[0101] [Preparation of powdered geopolymer composition]

[0102] Fly ash, various slag powders, soda ash and powdered sodium silicate were weighed according to the mixing table in Table 2, put into a polyethylene bag and stirred for 3 minutes, thereby preparing a powdered geopolymer composition in a uniformly dispersed state.

[0103] [Table 2]

[0104]

[0105] ※AL / W: The molar ratio of alkali metal elements (AL) to water (W) contained in soda ash or powdered sodium silicate.

[0106] ※Si / AL: The molar ratio of silicon (Si) to alkali metal elements (AL) contained in soda ash or powdered sodium silicate.

[0107] ※(AL+W) / P: Volume ratio of solution mixed with soda ash, powdered sodium silicate and water to fly ash and various slag powders.

[0108] (Comparative Example 1)

[0109] Comparative Example 1 is a mortar using ordinary Portland cement as a general-purpose material as a bonding material, and the formulation and mixing method thereof are in accordance with 11.5 of JIS R 5201:2015 (Physical testing methods for cement).

[0110] (Comparative Example 2)

[0111] Comparative Example 2 is a geopolymer composition obtained by using active fillers consisting of slag powder and fly ash that have not been subjected to carbonation treatment and heating treatment, and an alkali source consisting of soda ash, powdered sodium silicate and water.

[0112] (Comparative Examples 3 to 5)

[0113] Comparative Examples 3 to 5 are geopolymer compositions using slag powder (in the case of BFS-400, heating at 400°C for 3 hours) obtained by heat treatment described in Patent Document 1 and active filler consisting of fly ash, and alkali source consisting of soda ash and powdered sodium silicate. It should be noted that the contents of various slag powders, AL / W (molar ratio), Si / AL (molar ratio) and (AL+W) / P, which are believed to contribute to the usable time, compressive strength, and 15-beat mortar flow value (fluidity), are consistent with those in Comparative Example 2.

[0114] (Example 1)

[0115] Example 1 is a geopolymer composition using an active filler composed of carbonated slag powder (BFS-A) containing 1.26 mass % of CO2 and 0.58 mass % of bound water and fly ash, a powdered geopolymer composition as an alkali source composed of soda ash and powdered sodium silicate, and water. It should be noted that the contents of various slag powders, AL / W (molar ratio), Si / AL (molar ratio) and (AL+W) / P, which are considered to contribute to the usable time, compressive strength, and 15-beat mortar flow value (fluidity), are consistent with those of Comparative Examples 2 to 5.

[0116] (Examples 2 to 6)

[0117] Examples 2 to 6 are geopolymer compositions using active fillers composed of carbonated slag powder (BFS-B) and fly ash with increased CO2 and bound water content, and powdered geopolymer compositions composed of soda ash and powdered sodium silicate as alkali sources, and water. It should be noted that the contents of various slag powders, AL / W (molar ratio), and Si / AL (molar ratio) that are considered to contribute to the usable time, compression strength, and 15-beat mortar flow value (fluidity) are consistent with Comparative Examples 2 to 5, and (AL+W) / P is reduced in sequence in Examples 3 to 5.

[0118] [Mixing of mortar using geopolymer composition]

[0119] The powdered geopolymer composition and water were added to a Hobart mixer and stirred for 1 minute. 1350 g of aggregate was added and kneaded for 30 seconds. After scraping for 15 seconds, kneading was further performed for 2 minutes to obtain a uniformly kneaded hydraulic composition in the form of mortar. The 15-beat mortar flow rate value, usable time, and compressive strength of the obtained mortar were measured, and the results are shown in Table 3.

[0120] [15-beat mortar flow test]

[0121] According to the mortar flow test described in JIS A 5201, the mortar flow rate values ​​after applying 15 drops of motion were measured immediately after cooking of Comparative Examples 1 to 5 and Examples 1 to 6. The results are shown in Table 3.

[0122] [Determination of usable time]

[0123] At present, the method for determining the usable time has not been established. For the cement composition of Comparative Example 1, the mortar flow test described in JIS A5201 was implemented every 5 minutes to 30 minutes from just after mixing, and every 10 minutes after 30 minutes. The result was less than 130 mm after 120 minutes. Therefore, it was used as a criterion for determining whether it can be used. For Comparative Examples 1 to 5 and Examples 1 to 6, similarly, the test was implemented every 5 minutes to 30 minutes from just after mixing, and every 10 minutes after 30 minutes. The elapsed time until the flow value became less than 130 mm was determined as the usable time of the geopolymer composition. The results are shown in Table 3.

[0124] [Compression strength test]

[0125] The mortars of Comparative Examples 1 to 5 and Examples 1 to 6 were sealed into The containers (diameter) were 50 mm × 100 mm and sealed and cured at 20°C to the specified material age (1 day, 7 days and 28 days).

[0126] The mortars cured to predetermined material ages (1 day, 7 days, and 28 days) were subjected to a compression strength test in accordance with the compression strength test method described in JIS A1108 to measure the compression strength. The results are shown in Table 3.

[0127] [Table 3]

[0128]

[0129] ※The brackets in () indicate the ratio of the compressive strength to that of Comparative Example 2.

[0130] As shown in Table 3, in Comparative Examples 2 to 5, a tendency was observed that the compressive strength decreased significantly as the usable time increased.

[0131] When comparing Example 1 with Example 2, it is apparent that since both the amount of bound water and the amount of CO 2 are increased, the usable time can be extended while maintaining the strength.

[0132] In Examples 1 to 6, compared with Comparative Examples 2 to 5, a usable time of about 90 minutes or 120 minutes of working time, which is sufficient to meet the guidelines of the Japanese Society of Civil Engineers and the Japanese Society of Architects, was obtained, and the strength performance was 80% or more compared with the system using untreated slag fine powder. In addition, the flow rate value of 15-beat mortar also tends to be improved by carbonation treatment, and it can be seen that the workability of the geopolymer composition is also greatly improved.

[0133] Description of Reference Numerals

[0134] (1) CO2 gas cylinder

[0135] (2) Nozzle

[0136] (3) Constant temperature water tank

[0137] (4) Gas cleaning bottle

[0138] (5) Water

[0139] (6) Slag powder slurry

[0140] (7) Blender

[0141] (8) Dryer

[0142] (9) Heat-resistant container

[0143] (10) Carbonated slag powder slurry

Claims

1. A geopolymer composition comprising: an active filler comprising carbonated slag powder and pozzolanic material, an alkali source and water, The carbonated slag powder contains 0.1 mass % to 2.0 mass % of CO 2 and 0.26 mass % to 1.0 mass % of bound water.

2. The geopolymer composition according to claim 1, wherein The carbonated slag powder contains 1.0 mass % to 2.0 mass % of CO 2 and 0.5 mass % to 1.0 mass % of bound water.

3. The geopolymer composition according to claim 1, wherein: The carbonated slag powder contains 1.5 mass % to 2.0 mass % of CO 2 and 0.75 mass % to 1.0 mass % of bound water.

4. The geopolymer composition according to any one of claims 1 to 3, characterized in that The carbonated slag powder is obtained by subjecting the slag powder to a carbonation treatment under wet conditions in which 0.5 parts by mass or more of water is present relative to 1 part by mass of the slag powder.

5. A powdered geopolymer composition comprising: an active filler comprising carbonated slag powder and pozzolanic material powder; and a powdered alkali source comprising at least one selected from alkali metal silicate powder and alkali metal carbonate powder. The carbonated slag powder contains 0.1 mass % to 2.0 mass % of CO 2 and 0.26 mass % to 1.0 mass % of bound water.

6. The powdered geopolymer composition according to claim 5, characterized in that The alkali source is composed of alkali metal silicate powder and alkali metal carbonate powder.

7. The powdered geopolymer composition according to claim 5 or 6, characterized in that The alkali metal silicate powder is sodium silicate powder.

8. The powdered geopolymer composition according to claim 5 or 6, characterized in that The alkali metal carbonate powder is sodium carbonate powder.

9. A geopolymer composition comprising the powdered geopolymer composition of claim 5 or 6 and water.

10. A method for producing a geopolymer composition, comprising mixing the powdered geopolymer composition according to claim 5 or 6 with water.

11. A geopolymer hardened body, which is a hardened body of the geopolymer composition according to any one of claims 1 to 3.

12. A geopolymer hardened body, which is a hardened body of the geopolymer composition according to claim 9.