Article comprising graphite-containing composite material

By mixing and firing carbon black, flake graphite, needle coke and resin, composite products suitable for molten metal are prepared, which solves the problems of heavy weight, high cost or low quality of existing products and achieves high strength , non-wetting surface composites suitable for a variety of molten metal applications.

CN118871406APending Publication Date: 2024-10-29FOSECO INTERNATIONAL LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380026790.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-15
Filing Date
2023-03-11
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing cast iron, ceramic fiber vacuum formed products and reinforced fiber material products have problems such as excessive weight, high cost or low quality during molten metal processing, making it difficult to meet performance requirements.

Method used

By mixing carbon black, flake graphite, and needle coke with resin to form a granular mixture that is shaped and fired, composite articles with controlled porosity and graphite registration are produced, suitable for containing or processing molten metal.

Benefits of technology

The result is a high-strength, non-wetting surface and cost-effective composite article suitable for a variety of molten metal applications, including rotors, ladles, filters and crucibles, significantly reducing production costs and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036761240000211
    Figure BDA0005036761240000211
  • Figure HDA0005036761250000011
    Figure HDA0005036761250000011
  • Figure HDA0005036761250000021
    Figure HDA0005036761250000021
Patent Text Reader

Abstract

A method of forming an article comprising a graphite-containing composite material is disclosed. The article is suitable for containing or processing molten metal such as aluminum. The method includes forming at least one particulate mixture by mixing at least carbon black, flake graphite, needle coke with at least one resin, wherein the at least one resin has a flow distance of from 20 mm to 150 mm as measured by ISO 8619: 2003. The method further includes shaping the particulate mixture into a shaped body and firing the shaped body.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The present disclosure relates to methods of forming articles comprising composite materials containing graphite, and articles comprising composite materials containing graphite.

[0002] The manufactured products (such as refining vessels, transfer vessels, etc.) used in molten metal processing are traditionally made of cast iron, which results in heavy products that absorb heat. Ceramic fiber vacuum formed products have been developed to overcome the problems associated with their cast iron counterparts. However, such ceramic fiber formed products are difficult to meet basic performance requirements. Recently, enhanced fiber materials have been developed as substitutes for both cast iron and ceramic fiber vacuum formed products. However, the products made of reinforced fiber materials have high costs associated with them or have low quality. Therefore, it is necessary to provide manufactured products that can be used in molten metal applications and other applications, which overcome the problems associated with cast iron products, ceramic fiber vacuum formed products and products containing reinforced fiber materials. Summary of the invention

[0003] The present application provides a method for forming an article comprising a composite material containing graphite, wherein the article is suitable for containing or processing molten metal such as aluminum. The method comprises the following steps:

[0004] (a) forming at least one pelletized mixture by mixing at least carbon black, flake graphite, needle coke and at least one resin, wherein the resin has a flow distance of 20 mm to 150 mm as measured by ISO 8619:2003;

[0005] (b) shaping the at least one particulate mixture into at least one shaped body; and

[0006] (c) firing the at least one shaped body.

[0007] The present application provides a method for forming an article comprising a composite material containing graphite, which is suitable for containing or processing molten metals such as aluminum. Non-limiting examples of such articles are ladles, crucibles, filters, rotors and rotor subcomponents, continuous fiber wovens, mesh screens, machined parts, etc. The method of the present invention provides an article with desired and controlled porosity and graphite registration. In the remainder of this article, the terms "porosity" and "fine porosity" have the same meaning and can be used interchangeably. The method of the present disclosure also enables the formation of articles with high strength (e.g., composite materials have a flexural strength of about 10MPa to 25MPa or optionally higher) and non-wetting (i.e., non-stick) surfaces. These and other aspects of the present disclosure will now be described in more detail. DETAILED DESCRIPTION

[0008] The present disclosure will now be described in more detail by reference to the following discussion and accompanying drawings of the present disclosure. In the following description, many specific details, such as specific structures, parts, materials, sizes, processing steps and technologies are set forth, so as to provide an understanding of the various embodiments of the present disclosure. However, it will be appreciated by those skilled in the art that the various embodiments of the present disclosure may also be implemented without these specific details. As used throughout the present disclosure, the term "about" generally indicates ±10%, ±5%, ±2%, ±1% or ±0.5% of a certain numerical value. When a certain range is expressed in the present disclosure as from a numerical value to another numerical value (e.g., 20 to 40), the present disclosure considers any numerical value within the range (i.e., 22, 24, 26, 28.5, 31, 33.5, 35, 37.7, 39 or 40) or any amount defined by any one of two values ​​within the range (e.g., 28.5-35).

[0009] The terms used herein are used only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. As used herein, the singular forms "a / an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It will be further understood that when the terms "comprises / comprising" are used in the present disclosure, they specify the presence of stated features, wholes, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, parts and / or groups thereof.

[0010] In the context of the present invention, the expression "at least one X" is intended to mean one or more than one X. Mixtures of X can also be used for the purposes of the present invention.

[0011] For the situation that microparticle is spherical or substantially spherical, the particle size given herein can refer to diameter. For the situation that microparticle is substantially different from spherical, particle size is based on the equivalent diameter of microparticle. As known in the art, the term "equivalent diameter" is used to represent the size of the irregularly shaped object by the diameter of a sphere having the same volume as the irregularly shaped object, thereby representing the size of the object. Particle size can also be expressed as D50 particle size in this article, i.e. half of the microparticle is above the value represented, and the other half is below the value represented.

[0012] According to the present invention, the article is suitable for containing or processing molten metal. Non-limiting examples of such articles are rotors, ladles, filters, and crucibles or parts thereof. These articles are compatible with low-pressure and high-pressure die casting of molten metals, such as molten aluminum.

[0013] The method of the present invention comprises the step (a) of forming at least one pelletized mixture by mixing at least carbon black, flake graphite, needle coke and at least one resin, wherein the resin has a flow distance of 20 mm to 150 mm as measured by ISO 8619: 2003. Unless otherwise stated, the flow distance is measured at 125°C.

[0014] As used herein, the term "pellet mixture" refers to a blended mixture comprising at least carbon black, flake graphite, and needle coke and at least one resin.

[0015] The inventors have surprisingly found that carbon black, flake graphite, and needle coke provide complementary shape profiles that provide a high degree of compaction when a shaped body is formed from the particulate mixture. When the powders (i.e., carbon black, flake graphite, and needle coke) are mixed together with a resin that exhibits a flow distance as described above, a composite material containing graphite is obtained that performs well in terms of porosity, density, surface roughness, strength, and wettability.

[0016] The inventors have found, in particular, that the method of the present invention provides a composite material having a pore profile having a pore volume and a pore size distribution such that at least 95% of the total pore volume is contained in pores having a diameter or an equivalent diameter of less than 1 μm; in further embodiments or in the same embodiment, at least 40% of the pore volume of pores having a diameter or an equivalent diameter of less than 1 μm is contained in pores having a diameter or an equivalent diameter of less than 0.1 μm. The fine pore profile formed in the manufactured composite material enables a significant reduction in the achievable surface roughness of the composite material in the article. In the context of the present invention, the pore profile (pore diameter) is understood as porosity and is measured according to the ASTM C830-00 (2016) standard. The pore profile is measured by mercury (Hg) intrusion analysis. The equipment used for performing this analysis is an AutoPore V, The surface roughness R of the composite material obtained by the method of the present invention a The method of the invention allows obtaining a surface roughness R a Composite materials between 3.2 μm and 0.025 μm, where the surface roughness R a is as provided in the ISO 1302:1992 standard. The reduction in surface roughness also affects the adhesion (adhesion energy) or spreading (surface energy) and wetting (contact angle) forces generated between the molten metal and the manufactured article. This has an important impact on the performance of the manufactured article as a rotating object (e.g., a rotor) or as a stationary part (e.g., a crucible).

[0017] When an article is made (e.g., an article is manufactured) by the method according to the present invention, a substantially net-shaped article having a non-wetting surface is obtained. "Substantially net-shaped" means that the aspect (i.e., size and shape) of the article produced by the method of the present disclosure is close to (at least 90% or greater than) the desired aspect (size and shape) of the finished product or article. By forming a substantially net-shaped article, the production costs and time associated with the manufacture of the final product are greatly reduced.

[0018] By "non-wetting surface" is meant that the articles produced from the composite materials of the present disclosure will not be penetrated by molten / liquid metals (such as copper or aluminum, for example) even at high pressures P0. In graphite articles (such as containers for holding molten metals), penetration of molten metals can be achieved by applying a sufficiently high P0 to overcome the capillary pressure P0. C To achieve, where P C =-(2σ LV / r eff )cosθ, where σ LV is the surface energy of the liquid, r eff is the effective pore radius of the composite material, and θ is the contact angle of the pore wall. At the effective pore radius of the composite material of the present disclosure, the capillary pressure is too large to allow infiltration of the molten metal. Advantageously, in embodiments of the present disclosure, even after prolonged exposure to the molten metal or after repeated exposure to the molten metal, little or no article is corroded by the molten metal that penetrates through the pores.

[0019] The mixing step (i.e., step (a) as described in detail above) can be performed in different ways. For example, the granular mixture of the present disclosure can be prepared by first adding carbon black, flake graphite, needle coke, optionally one or more additives as defined below, and resin. The addition of the various components / raw materials can be performed in any order. For example, and in one embodiment, carbon black, flake graphite, needle coke, optionally one or more additives are added before adding the resin. In other embodiments, the resin is added first, and carbon black, flake graphite, needle coke are added afterwards. Mixing can be performed continuously during the addition of the various components / raw materials, or intermittently during the addition of the various components / raw materials. The amounts of the various components / raw materials used to provide the granular mixture are as specified below.

[0020] During mixing, the powder particles (i.e., carbon black, flake graphite, and needle coke) may be bound together by the resin to form particles. In this embodiment, mixing may also be referred to as granulation. Preferably, the particles may have a size of about 25 μm to about 4 mm, preferably a particle size of about 70 μm to about 700 μm.

[0021] In another embodiment, the process according to the present invention may further comprise a granulation step after the mixing step.

[0022] In one example, mixing includes high shear mixing of raw materials. In one example where a high shear mixing device is used in the mixing process, resin can help form or coat the raw material agglomerates. Mixing parameters can be changed to increase or decrease the size and distribution of particles as needed to optimize their use in subsequent processing steps. An example of a high shear mixer can be an Eirich mixer or the like. The mixing process forms a granular mixture of the present disclosure.

[0023] In some embodiments, the particulate mixture has a bimodal particle size distribution, wherein a first group of particles has a particle size diameter of about 50 μm to about 100 μm, and a second group of particles has a particle size diameter of about 110 μm to about 1000 μm. The first group of particles may constitute about 30 volume percent to about 60 volume percent of the total particulate mixture, and the second group of particles may constitute about 20 volume percent to about 40 volume percent of the total particulate mixture (as noted elsewhere in this disclosure, the particle sizes expressed herein are D50 particle sizes, i.e., half of the particles are above the value expressed, and the other half are below the value expressed).

[0024]

[0046] The various components (ie, raw materials) that may be used in the granulated mixtures of the present disclosure will now be described in additional detail.

[0025] The carbon black that can be used in the granular mixture of the present disclosure contains at least 99 weight percent carbon and has an ash content of 1 weight percent or less. Typically, the carbon content in the carbon black that can be used in the present disclosure is about 99.5 weight percent to about 100 weight percent. The shape of the carbon black that can be used in the present application is spherical or substantially spherical; there may be some shape irregularities that deviate from a completely spherical shape. The carbon black that can be used in the present disclosure has a particle size of about 10 μm to about 50 μm, preferably a particle size of about 25 μm to about 40 μm.

[0026] Advantageously, the carbon black is present in the pelletized mixture in an amount equal to or greater than 2 weight percent, preferably equal to or greater than 3 weight percent, more preferably equal to or greater than 5 weight percent relative to the total weight of the pelletized mixture.

[0027] Preferably, the upper limit of the amount of carbon black in the pelletized mixture is less than or equal to 15 weight percent, preferably less than or equal to 10 weight percent, more preferably less than or equal to 8 weight percent relative to the total weight of the pelletized mixture.

[0028] According to at least one embodiment, the carbon black is present in the granular mixture in an amount of about 5 weight percent to about 10 weight percent, preferably about 5 weight percent to about 8 weight percent, relative to the total weight of the granular mixture. In the range represented by the present invention, the present disclosure contemplates the use of any numerical value within the range, or any amount bounded by any of the two values. For example, the content of carbon black in the granular mixture can be 5 weight percent, 5.5 weight percent, 6 weight percent, 6.5 weight percent, 7 weight percent, 7.5 weight percent, 8 weight percent, 8.5 weight percent, 9 weight percent, 9.5 weight percent, 10 weight percent, or for example, 5.5 weight percent to 8.5 weight percent.

[0029] The needle coke that can be used in the granular mixture of the present disclosure contains at least 99 weight percent carbon and has a sulfur content of 1 weight percent or less. Typically, the carbon content of the needle coke that can be used in the present disclosure is about 99.5 weight percent to about 100 weight percent. The needle coke that can be used in the granular mixture of the present disclosure is an irregularly shaped needle coke. "Irregularly shaped needle coke" means (or has a fibrous, cylindrical or needle-like structure) evolved from a fibrous, cylindrical or needle-like structure. The needle coke that can be used in the present disclosure has a particle size of about 10 μm to about 50 μm, wherein a particle size of about 25 μm to about 40 μm is more typical.

[0030] The inventors have determined that needle coke exhibits similar toughness and increased thermal shock resistance compared to other types of carbon (such as, for example, chopped carbon fibers). The inventors have also determined that needle coke exhibits superior oxidation resistance compared to carbon fibers, and further, the use of needle coke (versus comparative carbon fibers) provides superior surface smoothness in a composite material comprising graphite when a shaped body is fired to provide a composite material comprising graphite. Thus, the surface smoothness of the composite material is improved by the use of needle coke.

[0031] Advantageously, the needle coke is present in the pelletized mixture in an amount equal to or greater than 0.5 weight percent, preferably equal to or greater than 1 weight percent, more preferably equal to or greater than 2 weight percent relative to the total weight of the pelletized mixture.

[0032] Preferably, the upper limit of the amount of needle coke in the pelletized mixture is less than or equal to 7 weight percent, preferably less than or equal to 5 weight percent, more preferably less than or equal to 4 weight percent, relative to the total weight of the pelletized mixture.

[0033] In a preferred embodiment of the present invention, the needle coke is present in the particulate mixture in an amount of about 1 weight percent to about 5 weight percent, preferably about 2 weight percent to about 4 weight percent, relative to the total weight of the particulate mixture.

[0034] The flake graphite that can be used in the granular mixture of the present disclosure contains at least 95 weight percent carbon and has an ash content of 1 weight percent or less. Typically, the carbon content of the flake graphite that can be used in the present disclosure is about 95 weight percent to about 99 weight percent. The flake graphite that can be used in the present disclosure has a particle size of about 10 μm to about 500 μm, with a particle size of about 25 μm to about 40 μm being more typical. In one embodiment, the flake graphite that can be used in the granular mixture of the present disclosure is a naturally occurring type of graphite that is typically in the form of discrete flakes; the discrete flakes may include hexagonal crystals; there may be some irregularities in the shape of the flake graphite crystals that deviate from a perfect hexagon. In one embodiment, the flake graphite that can be used in the granular mixture of the present disclosure has a distinct flake or plate-like morphology.

[0035] Advantageously, the flake graphite is present in the particulate mixture in an amount equal to or greater than 50 weight percent, preferably equal to or greater than 65 weight percent, more preferably equal to or greater than 75 weight percent relative to the total weight of the particulate mixture.

[0036] Preferably, the upper limit of the amount of flake graphite in the particulate mixture is less than or equal to 90 weight percent, preferably less than or equal to 85 weight percent, more preferably less than or equal to 80 weight percent relative to the total weight of the particulate mixture.

[0037] In a preferred embodiment of the present invention, flake graphite is present in the particulate mixture in an amount of about 65 weight percent to about 85 weight percent, preferably about 75 weight percent to about 80 weight percent, relative to the total weight of the particulate mixture.

[0038] In at least one embodiment, the generally hexagonal crystal morphology of flake graphite, the fibrous, cylindrical, needle-like or irregular shapes of needle coke, and the substantially spherical shape of carbon black provide complementary shape profiles that provide a high degree of compaction when a shaped body is formed from the particulate mixture.

[0039] Preferably, at least a portion of the carbon black has a generally spherical shape. Preferably, at least a portion of the needle coke has a generally cylindrical, fibrous or needle-like profile. Preferably, at least a portion of the flake graphite has a generally hexagonal or triangular profile.

[0040] According to the present invention, the resin has a button flow distance of 20 mm to up to 150 mm as measured by ISO 8619:2003. Those skilled in the art will be able to select an appropriate resin in order to obtain the required flow distance of the present invention. The inventors have surprisingly found that the granular mixture containing the resin of the present disclosure, which has a button flow distance of 20 mm to up to 150 mm as measured by ISO 8619:2003, reduces the complexity and number of steps in the mixing step compared to the binder systems of the prior art.

[0041] Advantageously, the resin has a Dome Flow Distance as measured by ISO 8619:2003 equal to or greater than 20 mm, preferably equal to or greater than 40, more preferably equal to or greater than 70 mm.

[0042] Preferably, the upper limit of the flow distance of the resin as measured by ISO 8619:2003 is less than or equal to 150 mm, preferably less than or equal to 70 mm, more preferably less than or equal to 40 mm.

[0043] In a preferred embodiment of the invention the resin has a Dome Flow Distance as measured by ISO 8619:2003 of 70 mm to up to 150 mm, preferably 40 mm to 70 mm, more preferably 20 mm to up to 40 mm.

[0044] In one embodiment of the method according to the present invention, the resin that can be used has a dome flow distance of 70mm to up to 150mm as measured by ISO 8619:2003. Resins with such flow distances can be described as "low molecular weight resins" in this article. In another embodiment of the present disclosure, the resin that can be used in the present disclosure has a dome flow distance of 40mm to 70mm as measured by ISO 8619:2003. Resins with such flow distances can be described as "medium molecular weight resins" in this article. In another embodiment of the present disclosure, the resin that can be used in the present disclosure has a dome flow distance of 20mm to up to 70mm as measured by ISO 8619:2003. Resins with such flow distances can be described as "high molecular weight resins" in this article. In some other embodiments of the present disclosure, any combination of low molecular weight resins, medium molecular weight resins, and high molecular weight resins can be used.

[0045] It should be noted that the type of resin (i.e., low, medium and high molecular weight resins as defined above) can be selected to control the overall viscosity of the binder system. It should be further noted that the type of resin (i.e., low, medium and high molecular weight resins as defined above) affects the strength of the green compact. For example, high molecular weight resins as defined herein provide the highest strength green compact (flexural strength higher than 2MPa), medium molecular weight resins as defined herein provide medium strength green compact (flexural strength of 1MPa to 2MPa), and low molecular weight resins as defined herein provide the lowest strength green compact (flexural strength lower than <1MPa). The green compact represents the granular mixture after molding and before firing.

[0046] It should be noted that the resins of the present disclosure aid in the granulation mixing step to form a granular mixture. The organic matter of the resin is typically removed during the firing process.

[0047] Preferably, a resin having a viscosity of about 9000 cps to about 30,000,000 cps is selected. More preferably, a resin having a viscosity of about 9000 cps to about 150,000 cps is selected. Unless otherwise stated, viscosity is measured at 25°C.

[0048] Advantageously, the resin is present in the granulated mixture in an amount equal to or greater than 2 percent by weight, preferably equal to or greater than 4 percent by weight, more preferably equal to or greater than 6 percent by weight relative to the total weight of the granulated mixture.

[0049] Preferably, the upper limit of the amount of the resin in the granular mixture is less than or equal to 15 weight percent, preferably less than or equal to 10 weight percent, more preferably less than or equal to 8 weight percent, relative to the total weight of the granular mixture.

[0050] In a preferred embodiment of the present invention, the resin is present in the granular mixture in an amount of about 2 weight percent to about 10 weight percent, preferably about 6 weight percent to about 8 weight percent, relative to the total weight of the granular mixture.

[0051] In the context of the present invention, the resin may be in various physical states, preferably, the resin is in a liquid state.

[0052] Preferably, the resin is a thermosetting resin.

[0053] The selection of resin is advantageously determined by having a high carbonization rate after pyrolysis. Table 1 below lists typical carbonization rates after pyrolysis of various carbon source materials. Preferably, the resin provides a high carbonization rate of equal to or greater than 40 weight percent, or equal to or greater than 50 weight percent, or equal to or greater than 60 weight percent after pyrolysis.

[0054] Table 1

[0055] Carbon source Typical char yield after pyrolysis wt% Coal tar pitch 45-55 Phenolic resin 40-70 Furan resin 45-60 Polyacrylonitrile (PAN) cellulose 35-45 Epoxy resin 25-35 Unsaturated polyester resin 15-25 Polypropylene (PP) <2 Polyethylene terephthalate (PET) <0.5

[0056] As will be appreciated by those skilled in the art, when the shaped body is fired to high temperatures, the amorphous carbon (i.e., the amorphous carbon produced by the conversion of the resin when the shaped body is fired to provide a composite material comprising graphite) can be further reconstituted into other forms of carbon, such as, for example, crystalline carbon in the form of carbon nanotubes, graphene, and similar other materials.

[0057] Advantageously, the resin is selected from the group consisting of phenolic resins, cellulose-based derivatives, siloxane-modified resins, modified epoxy resins, polyimides, benzoxazines, or any combination thereof. Non-limiting examples of commercial polyimides are ZT1000 [polyimide] and Cornerstone (18C021). Non-limiting examples of commercial benzoxazines are Huntsman (18B028). In some embodiments, the resin additionally comprises additives such as carbores. More preferably, the resin is a phenolic resin. One advantage of using a phenolic resin is that up to 70 wt % of the phenolic resin can be converted into carbon in the form of amorphous carbon, for example when the molded body is fired to provide a composite material comprising graphite.

[0058] In a preferred embodiment of the present invention, the resin can be formed by condensation of phenol or phenol derivatives with aldehydes, especially formaldehyde, in the presence of a catalyst. In one embodiment of the present disclosure, the phenolic resin that can be used in the present disclosure has a dome flow distance of 70 mm to up to 150 mm as measured by ISO 8619:2003. The phenolic resin with such a flow distance can be described as a "low molecular weight phenolic resin" in this article. In another embodiment of the present disclosure, the phenolic resin that can be used in the present disclosure has a dome flow distance of 40 mm to 70 mm as measured by ISO 8619:2003. The phenolic resin with such a flow distance can be described as a "medium molecular weight phenolic resin" in this article. In another embodiment of the present disclosure, the phenolic resin that can be used in the present disclosure has a dome flow distance of 20 mm to up to 70 mm as measured by ISO 8619:2003. The phenolic resin with such a flow distance can be described as a "high molecular weight phenolic resin" in this article. In one example, the phenolic resin that can be used in the present disclosure is a commercially available phenolic resin known as Sumitomo XF3011P. In another embodiment of the present disclosure, the phenolic resin used is a liquid phenolic resin. In some other embodiments of the present disclosure, any combination of low molecular weight phenolic resin, medium molecular weight phenolic resin, high molecular weight phenolic resin, or liquid phenolic resin can be used.

[0059] According to at least one embodiment, in order to further improve the fluidity and / or viscosity of the resin, at least one solvent may be added to the resin. In this embodiment, the resin may also be referred to as an adhesive system, which is composed of at least one resin and at least one solvent. It should be noted that the type of resin and the type of solvent may be selected to control the overall viscosity of the adhesive system. According to at least one embodiment, the solvent comprises a dibasic ester. In one embodiment, the solvent may be a dibasic ester having the formula CH3O2C(CH2) n Esters of dicarboxylic acids of CO2CH3, wherein n is equal to 2, 3 or 4. In some embodiments, the solvent used is an acetate. In other embodiments, the acetate is propylene glycol diacetate. Other solvents are possible and can be used in combination with the resin as a binder system of the present disclosure. According to an embodiment of the present disclosure, the resin and the solvent are present in the granular mixture in a weight ratio of about 1:1 to about 6:1. According to another embodiment of the present disclosure, the resin and the solvent are present in the granular mixture in a weight ratio of about 2:1 to about 4:1.

[0060] When the resin further comprises a solvent, the solvent is present in the granular mixture in an amount of about 1 weight percent to about 5 weight percent, preferably about 3 weight percent to about 4 weight percent, relative to the total weight of the granular mixture.

[0061] In some embodiments, the resin of the granular mixture additionally comprises an optional binder plasticizer. Thus, in some embodiments, the resin may further comprise a binder plasticizer, such as, for example, dextrin, propylene carbonate, stearic acid, oleic acid, glycol and / or triacetin; in other embodiments, no binder plasticizer is used.

[0062] In some embodiments, the granular mixture of the present disclosure does not contain any intentionally added water. In yet other embodiments, water may be included in the granular mixture of the present disclosure. In some embodiments of the present disclosure, the granular mixture has a moisture content of less than about 5.0 weight percent, preferably equal to or less than 4.0 weight percent, more preferably equal to or less than 3.0 weight percent relative to the total weight of the granular mixture. Advantageously, the granular mixture has a moisture content equal to or greater than 0.5 weight percent, preferably equal to or greater than 1 weight percent, more preferably equal to or greater than 2.0 weight percent relative to the total weight of the granular mixture. In an example, the moisture content of the granular mixture is about 1.0 weight percent to 4.0 weight percent relative to the total weight of the granular mixture.

[0063] According to at least one embodiment, carbon black, flake graphite, needle coke and resin provide 100% of the total weight of the pelletized mixture. In this embodiment, the pelletized mixture is composed entirely of carbon black, flake graphite, needle coke and resin; no other components / additives are used in providing the pelletized mixture. This embodiment can be advantageously used to manufacture articles in which the presence of other foreign substances besides carbon is undesirable, such as, for example, crucibles used in the manufacture of synthetic graphite.

[0064] In one embodiment, the pelletized mixture comprises about 6 weight percent, 6.2 weight percent, 6.4 weight percent, 6.6 weight percent, 6.8 weight percent, 7 weight percent, 7.2 weight percent, 7.5 weight percent, or in a range defined by any two of the foregoing values ​​of carbon black, about 1 weight percent, 1.2 weight percent, 1.4 weight percent, 1.6 weight percent, 1.8 weight percent, 2 weight percent, 2.2 weight percent, 2.5 weight percent, or in a range defined by any two of the foregoing values ​​of needles. The granular mixture further comprises about 3.8 weight percent, 4 weight percent, 4.2 weight percent, 4.5 weight percent, or a range defined by any two of the foregoing values, of a granular coke, about 78 weight percent, 78.2 weight percent, 78.4 weight percent, 78.6 weight percent, 78.8 weight percent, 79 weight percent, 79.2 weight percent, 79.5 weight percent, or flake graphite within a range defined by any two of the foregoing values, and about 7 weight percent, 7.2 weight percent, 7.4 weight percent, 7.6 weight percent, 7.8 weight percent, 8 weight percent, 8.2 weight percent, 8.4 weight percent, or a range defined by any two of the foregoing values, of a resin. When the granular mixture further comprises a solvent, and about 3 weight percent, 3.2 weight percent, 3.4 weight percent, 3.6 weight percent, the granular mixture further comprises about 3.8 weight percent, 4 weight percent, 4.2 weight percent, 4.5 weight percent, or a range defined by any two of the foregoing values, of a solvent.

[0065] In other embodiments, the granular mixture further comprises one or more of the following: antioxidant additives, toughening / strength enhancing additives, wear / erosion resistant agents, thermal insulation enhancing agents, and transition metals selected from Groups 4 to 12 of the Periodic Table of Elements. These additives may be in the form of powders or granules.

[0066] According to at least one embodiment, the granular mixture further comprises about 5 weight percent to about 15 weight percent, preferably about 8 weight percent to about 12 weight percent of an antioxidant additive relative to the total weight of the granular mixture. According to at least one embodiment, the antioxidant additive comprises boron carbide, silicon carbide, aluminum zinc phosphate, or any combination thereof.

[0067] The antioxidant additive is used to reduce the oxidation of the resulting composite material, while plugging holes and increasing the apparent density of the resulting composite material. Exemplary antioxidant additives that may be present in the granular mixture of the present disclosure include, but are not limited to, boron carbide, silicon carbide, bentonite, aluminum zinc phosphate, or any combination thereof. In one embodiment, relative to the gross weight of the antioxidant additive, the antioxidant additive comprises a mixture of the following: about 2 weight percent to about 7 weight percent boron carbide, about 1 weight percent to about 5 weight percent silicon carbide, about 0.25 weight percent to about 0.75 weight percent bentonite, and about 2 weight percent to about 5 weight percent aluminum zinc phosphate.

[0068] In some embodiments where boron carbide is used as an antioxidant additive, the boron carbide is provided in the form of fine particles having a particle size of less than about 50 μm, preferably a particle size in the range of about 25 μm to about 40 μm. In some embodiments where silicon carbide is used as an antioxidant additive, the silicon carbide is provided in the form of fine particles having a particle size of less than about 50 μm, preferably a particle size in the range of about 20 μm to about 40 μm. In some embodiments where bentonite is used as an antioxidant additive, the bentonite is provided in the form of fine particles having a particle size of less than about 10 μm, preferably a particle size in the range of about 1 μm to about 7 μm. In various embodiments, the boron carbide, silicon carbide, and bentonite may be in the form of powders or granules.

[0069] In some embodiments, the addition of antioxidant can be carried out in two separate or different stages. In embodiments in which the antioxidant addition is carried out in two stages, during the first stage of the two stages, the first stage antioxidant additive is added to the granular mixture. The granular mixture is then formed into a molded body consisting of the granular mixture. In the second stage of the two stages, the second stage antioxidant additive is applied to a portion or all of one or more exposed surfaces of the molded body, and the molded body is subsequently fired to provide a composite material consisting of graphite. In some embodiments, the first stage antioxidant additive added in the first stage is a different material from the second stage antioxidant additive added in the second stage. In some embodiments, the first stage antioxidant additive added in the first stage is the same material as the second stage antioxidant additive added in the second stage.

[0070] According to at least one embodiment, the granular mixture further comprises about 1 weight percent to about 5 weight percent, preferably about 2.5 weight percent to about 4.5 weight percent of a toughening / strength enhancing additive relative to the total weight of the granular mixture. According to at least one embodiment, the toughening / strength enhancing additive comprises carbon fiber, chopped carbon fiber bundles, basalt bundles, aluminum silicate fibers, chopped steel fibers, or any combination thereof.

[0071] Toughening / strength enhancing additives are used to increase the toughness and / or strength of the resulting composite material. Exemplary toughening / strength enhancing additives that may be present in the granular mixture of the present disclosure include, but are not limited to, carbon fibers, chopped carbon fiber bundles, basalt bundles, aluminum silicate fibers, chopped steel fibers, or any combination thereof. In some embodiments, the toughening / strength enhancing additive comprises carbon fibers, chopped carbon fiber bundles, or a combination thereof; such toughening / strength enhancing additives increase the toughness of the resulting manufactured article made from the granular mixture of the present application. In some embodiments, the toughening / strength enhancing additive comprises basalt, aluminum silicate fibers, or a combination thereof; such toughening / strength enhancing additives improve the strength of the resulting manufactured article made from the granular mixture of the present application and reduce its thermal conductivity. In some embodiments, the toughening / strength enhancing additive comprises chopped steel fibers; such toughening / strength enhancing additives increase the strength and toughness of the resulting manufactured article made from the granular mixture of the present disclosure.

[0072] According to at least one embodiment, the granular mixture further comprises about 1 weight percent to about 10 weight percent, preferably about 4.5 weight percent to about 8.5 weight percent of a wear / erosion resistant agent relative to the total weight of the granular mixture. According to at least one embodiment, the wear / erosion resistant agent comprises a metal oxide, a metal nitride, a metal boride, or any combination thereof.

[0073] Wear / erosion resistant agents are used to increase the wear of the resulting composite material and / or reduce the erosion of the composite material. Illustrative examples of wear / erosion resistant agents that can be used in the present application include metal oxides (such as zirconium oxide, or yttrium oxide), metal nitrides (such as boron nitride, aluminum nitride, or silicon nitride), metal borides (such as titanium diboride), or any combination thereof. In some embodiments, zirconium oxide is used as a wear / erosion resistant agent. In such embodiments, zirconium oxide can form zirconium silicide or zirconium silicate in situ, which can result in strong bonding, high oxygen resistance, high wear / erosion resistance and / or very fine pore profiles. In such embodiments, zirconium oxide can form zirconium boride with abnormally high wear / erosion resistance. Wear / erosion resistant agents that can be used in the present disclosure are typically nano-micron-sized powders with a particle size less than about 40 μm, with particle sizes ranging from about 5 μm to about 25 μm being more common.

[0074] According to at least one embodiment, the granular mixture further comprises an insulation enhancer of about 1 weight percent to about 5 weight percent, preferably 2.5 weight percent to 4 weight percent, relative to the total weight of the granular mixture. These agents provide improved thermal insulation for the resulting composite material. Illustrative examples of insulation enhancers that can be used in the present disclosure include, but are not limited to, colloidal silica pellets, fibers, or mixtures thereof. According to at least one embodiment, the insulation enhancer comprises colloidal silica pellets, fibers, or mixtures thereof. According to at least one embodiment, the insulation enhancer comprises a mixture of sodium aluminosilicate pellets and chopped silica fibers. According to at least one embodiment, optionally, the insulation enhancer comprises colloidal silica pellets, preferably aluminum colloidal silicate pellets; fibers, preferably a mixture of sodium and chopped silica fibers; or a mixture thereof. In such an embodiment, the mixture may comprise about 5 weight percent to about 50 weight percent of sodium aluminosilicate pellets and about 20 weight percent to about 70 weight percent of chopped silica fibers relative to the total weight of the insulation enhancer.

[0075] According to at least one embodiment, the granular mixture further comprises about 1 weight percent to about 5 weight percent, preferably 2.5 weight percent to about 4 weight percent of a transition metal selected from Groups 4 to 12 of the periodic table of elements relative to the total weight of the granular mixture. The transition metal can be used to add specific functions (such as catalytic functions) to the resulting composite material. Illustrative examples of suitable transition metals that can be used in the present disclosure include, but are not limited to, iron, titanium, nickel, or any combination thereof.

[0076] In some embodiments, clay may also be present in the granulated mixture of the present disclosure; when present, the clay is preferably present in an amount of about 0.25 weight percent to about 0.75 weight percent relative to the total weight of the granulated mixture.

[0077] In embodiments where the mixing step provides particles and the particulate mixture contains toughening / strength enhancing additives as defined above, wear / erosion resistant agents as defined above, thermal insulation enhancing agents as defined above, transition metals as defined above, or any combination thereof, these additives may be located (dispersed) within the particles of the particulate mixture, or these additives may be located between the particles of the particulate mixture.

[0078] According to at least one embodiment, the granular mixture as previously detailed consists essentially of particles, and wherein the toughening / strength enhancing additive, the wear / erosion resistant agent, the thermal insulation enhancing agent, the transition metal selected from Group 4 to Group 12 of the Periodic Table of Elements, or any combination thereof, is located within the particles. According to at least one embodiment, the granular mixture as previously detailed consists essentially of particles, and wherein the toughening / strength enhancing additive, the wear / erosion resistant agent, the thermal insulation enhancing agent, the transition metal selected from Group 4 to Group 12 of the Periodic Table of Elements, or any combination thereof, is located between the particles of the granular mixture.

[0079] In some embodiments of the present disclosure, the granular mixture comprises about 5 weight percent to about 10 weight percent carbon black, about 65 weight percent to about 85 weight percent flake graphite, about 1 weight percent to about 5 weight percent needle coke, about 2 weight percent to about 10 weight percent phenolic resin, and about 1 weight percent to about 5 weight percent solvent. In still other embodiments, the granular mixture comprises about 5 weight percent to about 8 weight percent carbon black, about 75 weight percent to about 80 weight percent flake graphite, about 2 weight percent to about 4 weight percent needle coke, about 6 weight percent to about 8 weight percent phenolic resin, and about 3 weight percent to about 4 weight percent solvent. In the ranges indicated above, the present disclosure contemplates the use of any numerical value within the range, or any amount bounded by any of the two values. For example, the carbon black content in the pelletized mixture can be 5 weight percent, 5.5 weight percent, 6 weight percent, 6.5 weight percent, 7 weight percent, 7.5 weight percent, 8 weight percent, 8.5 weight percent, 9 weight percent, 9.5 weight percent, 10 weight percent, or for example, 5.5 weight percent to 8.5 weight percent.

[0080] After forming the granular mixture (i.e., step (a) as previously detailed), the granular mixture is formed into a shaped body (i.e., step (b)); the shaped body may be referred to as a green body. Forming may include, but is not limited to, isostatic pressing (i.e., isostatic pressing), hydraulic pressing, extrusion, molding, or 3D printing. In some embodiments, the forming may be determined by the amount of resin present in the granular mixture. For example, 4 wt.% to 8 wt.% of the resin in the granular mixture may be advantageous for isostatic pressing or hydraulic pressing; 8 wt.% to 12 wt.% of the resin may be advantageous for extrusion; and 12 wt.% to 17 wt.% of the resin may be advantageous for 3D printing. In some embodiments, forming the granular mixture into a shaped body includes the following steps: machining or final shaping the granular mixture to form a rotor component; forming the granular mixture into a ladle; forming the granular mixture to form a crucible, and extruding or 3D printing the granular mixture to form a crucible. In one example, the granular mixture may be subjected to isostatic pressing using a shaped polyurethane bag pressed against a metal mandrel. The shaped body can include any shape, including, for example, the shape of a rotor or rotor component, a ladle, a crucible, and a molten metal filter or filter component. In some embodiments, the shaped body can be formed on a prefabricated structure before firing, such as, for example, a steel mesh, a filter or filter component, and a continuous carbon fabric.

[0081] The inventors have found that the process of the present invention provides a shaped body having a green strength of about 1 MPa to about 5 MPa flexural strength, about 1.5 g / cm 3 To about 1.7g / cm 3 The green density is about 0.5g / cm 3 To about 0.7g / cm 3 In the present disclosure, green strength can be measured by a 3-point bend test of a test piece (e.g., to measure flexural strength), green density can be measured by volume and weight measurements of a test piece, and powder packing density can be measured by measuring the weight of the powder filling a container of known volume. As used herein, "green strength" can refer to the strength of a material when it is processed to form its ultimate breaking strength. As used herein, "green density" is the density of a molded body before any heat treatment.

[0082] Preferably, when the shaping is isostatic pressing (i.e., isostatic pressing), during the mixing step (i.e., step (a) as described in detail above), the powder particles (i.e., carbon black, flake graphite and needle coke) can be bound together by the resin, thereby forming granules. In this embodiment, mixing can also be referred to as granulation.

[0083] In some embodiments, the shaped body may comprise a crucible shape, wherein the crucible shape is composed of a plurality of crucible rings which are uniformly stacked on top of each other to provide the crucible shape. The crucible ring is preferably obtained by final shaping of the granular mixture into a precise ring shape, or shaping of the granular mixture into a large crucible shape, cutting the large crucible shape into crucible rings and machining the crucible rings. This shaping is particularly advantageous because it allows partial replacement of the crucible without having to replace the entire crucible, thereby increasing repair time, reducing costs and improving overall efficiency.

[0084] In some embodiments, the molded body can be cured before firing. Curing the molded body before firing causes crosslinking of the resin, which allows improved handling and processing of the molded body before firing. Curing can be carried out in air before firing. Curing can be carried out at a single curing temperature, or various curing temperatures can be used. In one embodiment of the present disclosure, curing is carried out at a temperature of about 200° C. to about 300° C. and lasts for a period of about 1 to about 5 hours. Other curing temperatures and / or times can be used in the present disclosure. Curing can be carried out in any curing device commonly used in the art.

[0085] In some embodiments of the present disclosure, the molded body may undergo a coating process, a glazing process, an injection process, an infiltration process, or any combination thereof prior to firing. The coating process, the glazing process, the injection process, and / or the infiltration process may be performed directly on the molded body, or such processes may be performed on a molded body that has first undergone curing.

[0086] When the coating process is performed, at least a portion of the cured or uncured molded body may be coated with any suitable coating material using any well-known coating technique (e.g., such as spraying, dipping, brushing, etc.). In some embodiments, a silicon carbide (SiC), aluminum oxide, or aluminum titanate coating may be formed on at least a portion of the cured or uncured molded body. In some embodiments, a boron nitride coating may be formed on at least a portion of the cured or uncured molded body. The coating may change the porosity and / or finish of the composite material.

[0087] When the glazing process is performed, at least a portion of the cured or uncured molded body can be glazed with any suitable glazing material using any well-known glazing technique (e.g., spraying, dipping, brushing, etc.). In one example, a glazing material formulated from a glass-based composition can be used.

[0088] When the injection process is performed, any well-known injection process (such as roller injection, step-by-step injection and immersion injection) can be used to inject the material into at least a portion of the solidified or unsolidified and formed body. In one example, the borax mixture can be injected into at least a portion of the solidified and / or unsolidified molded body before firing. In one embodiment, at least a portion of the molded body composed of the granular mixture is coated with the injection material (e.g., an antioxidant additive), and the molded body is subsequently fired, wherein the injection material (e.g., an antioxidant additive) is injected into the composite material composed of graphite obtained by firing the molded body.

[0089] When the infiltration process is performed, any well-known infiltration technique (such as injection, chemical vapor infiltration, etc.) can be used to infiltrate at least a portion of the cured or uncured molded body with any suitable material. Preferably, before or after the firing step, at least a portion of the cured or uncured molded body is infiltrated with siloxane, a selected phosphate solution, or any combination thereof. In one example, a siloxane precursor, a selected phosphate solution, or any combination thereof can be infiltrated into at least a portion of the molded body before firing. In some embodiments, before or after the firing step, at least a portion of the composite material is infiltrated with siloxane, a selected phosphate solution, or any combination thereof. In one example, a siloxane precursor, a selected phosphate solution, or any combination thereof can be infiltrated into at least a portion of the composite material after firing. In one embodiment, at least a portion of a molded body consisting of a granular mixture is infiltrated with an infiltration material (e.g., an antioxidant additive), and the molded body is subsequently fired, wherein the infiltration material (e.g., an antioxidant additive) is infiltrated into a composite material containing graphite obtained by firing the molded body.

[0090] Next, the molded body is fired to provide a composite material comprising graphite (i.e., step (c)). Firing a molded body containing a granular mixture of the present disclosure provides a composite material comprising graphite. The composite material can also be an article composed of the composite material. Alternatively, the composite material can further undergo a manufacturing step to provide an article comprising the composite material. The article can be composed of a plurality of composite materials, which are stacked together to provide the article. For example, when the article is a crucible, the crucible can be composed of a plurality of crucible rings, which are evenly stacked on top of each other to provide the crucible. Alternatively or additionally, the composite material can undergo a coating process, a glazing process, an injection process, and / or an infiltration process to provide the article. Non-limiting examples of such articles include rotors, ladles, filters, and crucibles or parts thereof.

[0091] The inventors have found that the process of the present invention provides a composite material comprising graphite having improved properties, such as a porosity of about 10% to about 25%. Furthermore, the composite material obtained by the process of the present invention has a porosity of about 1.6 g / cm 3 To about 1.92g / cm 3 The apparent density of the composite material is preferably 1.5 Å. Advantageously, the composite material has a total pore volume and a pore size distribution in which at least 95% of the total pore volume is contained in pores having a diameter or an equivalent diameter of less than 1 μm, and at least 40% of the pore volume of pores having a diameter or an equivalent diameter of less than 1 μm is contained in pores having a diameter or an equivalent diameter of less than 0.1 μm. The fine pore profile formed in the composite material in the manufactured article makes it possible to significantly reduce the obtainable surface roughness of the composite material in the article. Regarding the surface roughness R of the composite material obtained by firing the molded body a , ISO 1302:1992 provides a method for indicating surface roughness. In practice, the average roughness (R a ) is often used in industry as a measure of surface smoothness. Using the method of the present invention, it is possible to obtain the surface roughness R a Composite materials between 3.2 μm and 0.025 μm, where the surface roughness R a is as provided in the ISO 1302:1992 standard. The reduction in surface roughness also affects the adhesion (adhesion energy) or spreading (surface energy) and wetting (contact angle) forces generated between the molten metal and the manufactured article. This has an important impact on the performance of the manufactured article as a rotating object (e.g., a rotor) or as a stationary part (e.g., a crucible).

[0092] Furthermore, according to the present invention, it is possible to provide an article (eg, an article of manufacture) which is a substantially final-shaped article and has a non-wetting surface as previously described.

[0093] Firing can be carried out at a single firing temperature, or various firing temperatures can be used. In one embodiment, firing is carried out at a temperature of about 800°C to about 1500°C. In one embodiment, the firing temperature is between 800°C-1300°C. In one embodiment, the firing temperature is about 1250°C to about 1300°C, preferably about 1000°C to about 1250°C. In one embodiment, the firing temperature is about 1400°C to about 1500°C. In one embodiment, the firing temperature is about 1250°C. In one embodiment, the firing temperature is about 1050°C.

[0094] The time period of firing can vary depending on the temperature of the firing process and the exact composition of the molded body. In one example, and at a temperature of about 1250° C. to about 1500° C., firing can be performed for a period of 5 hours to 50 hours, including the time and holding time of ramping up to the peak temperature. Firing can be performed under various ambient conditions, such as, for example, in a reducing environment or in a carbon environment (such as, for example, carbon monoxide). The carbon environment can be mixed with an inert carrier gas (i.e., helium, argon, and / or nitrogen).

[0095] Various firing profiles may be used in the present disclosure. In one example, the firing of the glazed formed body may be conducted in a reducing atmosphere at a temperature of about 1250°C to about 1300°C. In another example, and for glazed / coated formed bodies, firing in air at a temperature of about 1000°C to about 1250°C may be employed. In further examples, the coated or uncoated formed body may be fired in a reducing atmosphere at a temperature of about 1400°C to about 1500°C.

[0096] In some embodiments, a firing stage antioxidant additive (which may be alternatively referred to herein as a second stage antioxidant additive) may be added to the molded article during the firing process. Illustrative examples of firing stage antioxidant additives that may be used in the present disclosure include, but are not limited to, bentonite, zinc phosphate, aluminum phosphate, zinc aluminum phosphate, or any combination thereof. The firing stage antioxidant additive may be added in an amount of about 1 weight percent to about 6 weight percent, with the range of about 2 weight percent to about 4 weight percent being more common. In some embodiments, the firing stage antioxidant additive is the only antioxidant additive present. In other embodiments, the firing stage antioxidant additive is used in combination with an antioxidant additive added to form a granular mixture. In such embodiments, the antioxidant additive added to form a granular mixture may be referred to as a first stage antioxidant additive group, which includes boron carbide, silicon carbide, bentonite, zinc aluminum phosphate, or any combination thereof as defined above, and the firing stage antioxidant additive may be referred to as a second stage antioxidant additive group, which is different from the first antioxidant additive group and includes bentonite, zinc phosphate, aluminum phosphate, zinc aluminum phosphate, or any combination thereof.

[0097] In various embodiments, firing of a shaped body (containing a particulate mixture of the present disclosure) provides a composite material containing graphite having a fine pore profile, wherein at least 95% of the total pore volume is contained in pores having a diameter less than 1 μm, and at least 40% of the pore volume of pores having a diameter less than 1 μm is contained in pores having a diameter less than 0.1 μm. The fine pore profile formed in the composite material of the present disclosure results in excellent surface smoothness of the composite material or an article formed from the composite material. Regarding the surface roughness R of the composite material produced by firing the shaped bodya , ISO 1302:1992 provides a method for indicating surface roughness. In practice, the average roughness (R a ) is often used in industry as a measure of surface smoothness.

[0098] In some embodiments of the present disclosure, the method of the present invention further comprises a step of coating, glazing, injecting, infiltrating, or any combination thereof as described above before or after the firing step. Preferably, when a coating step is provided, at least a portion of the composite material is coated with a coating. In other words, at least a portion of the surface of the composite material is coated with a coating. Advantageously, the coating is at least one coating selected from the group consisting of boron nitride, silicon carbide, aluminum oxide, or aluminum titanate.

[0099] According to at least one embodiment, when an infiltration step is provided, at least a portion of the composite material is infiltrated with siloxane, a selected phosphate solution, or any combination thereof, before or after the firing step.

[0100] In another aspect of the present disclosure, a composite material comprising graphite is provided. In addition, an article comprising the composite material comprising graphite is provided. As described above, the composite material can also be an article consisting of the composite material. Alternatively, the composite material can further undergo a manufacturing step to provide an article comprising the composite material. Non-limiting examples of such articles include rotors, ladles, filters, and crucibles or parts thereof. In a preferred embodiment of the present invention, the article is a crucible, which is composed of a plurality of crucible rings, which are evenly stacked on top of each other to provide the crucible. Alternatively or additionally, the composite material can further undergo a coating process, a glazing process, an injection process and / or an infiltration process to provide the article.

[0101] The composite material has a total pore volume and a pore size distribution, wherein at least 95% of the total pore volume is contained in pores having a diameter or an equivalent diameter of less than 1 μm, and at least 40% of the pore volume of pores having a diameter or an equivalent diameter of less than 1 μm is contained in pores having a diameter or an equivalent diameter of less than 0.1 μm. Preferably, the composite material has a total pore volume and a pore size distribution, wherein at least 97% of the total pore volume is contained in pores having a diameter of less than 1 μm, and at least 40% of the pore volume of pores having a diameter of less than 1 μm is contained in pores having a diameter of less than 0.1 μm.

[0102] This hole profile can be Figure 1, entitled 'Pore size in fired graphite mixture'. The fine pore profile formed in the composite material in the manufactured article enables a significant reduction in the achievable surface roughness of the composite material in the article. The reduction in surface roughness also affects the adhesion (adhesion energy) or spreading (surface energy) and wetting (contact angle) forces generated between the molten metal and the manufactured article. This has an important impact on the performance of the manufactured article as a rotating object (e.g., a rotor) or as a stationary part (e.g., a crucible).

[0103] It is further understood that all definitions and preferences as described above apply equally to composite materials and articles comprising graphite.

[0104] Preferably, the composite material has a porosity of about 10% to about 25%, more preferably about 15% to about 20%.

[0105] Preferably, the composite material has a thickness of about 1.6 g / cm 3 To about 1.92g / cm 3 , more preferably about 1.7 g / cm 3 To about 1.8g / cm 3 The apparent density of .

[0106] In some embodiments, the composite material of the present disclosure has a porosity of about 15% to about 20%, a porosity of about 1.7 g / cm 3 To about 1.8g / cm 3 A density, and a certain total pore volume and pore size distribution, wherein at least 97% of the total pore volume is contained in pores with a diameter less than 1 μm, and at least 40% of the pore volume of pores with a diameter less than 1 μm is contained in pores with a diameter less than 0.1 μm.

[0107] Preferably, the composite material of the present invention comprises graphite in an amount of at least 65 weight percent, preferably at least 75 weight percent, and more preferably at least 85 weight percent relative to the total weight of the composite material. In some embodiments, the composite material of the present invention comprises graphite in an amount of about 65 weight percent to about 85 weight percent, preferably about 75 weight percent to about 80 weight percent relative to the total weight of the composite material.

[0108] According to at least one embodiment, the composite material has a surface roughness R between 3.2 μm and 0.025 μm. a , where the surface roughness R a As provided in ISO 1302:1992 standard.

[0109] Table 2 below provides the equivalent values ​​of Ra and N values ​​specified in ISO 1302:1992. Table 2 further provides the Ra values ​​in microinches or μin. under the ANSI B46.1 standard which is optionally used in the United States.

[0110] Table 2

[0111]

[0112] The following are some exemplary N value descriptions provided according to ISO 1302:1992: N = 10 (N10 = 12.5 μm) indicates rough turning with visible tool marks; N = 8 (N8 = 3.2 μm) indicates a smooth machined surface; N = 7 (N7 = 1.6 μm) indicates a static fit surface (or reference); N = 6 (N6 = 0.8 μm) indicates a bearing surface; and N = 1 (N1 = 0.025 μm) indicates a very finely ground surface. In various embodiments, the surface roughness (Ra) value of the composite material of the present disclosure is a value between N = 8 (N8 = 3.2 μm) and N = 1 (N1 = 0.025 μm). In at least one embodiment, the "pressed" surface finish of the composite material of the present disclosure varies between N=8 (3.2 μm) and N=1 (N1=0.025 μm); in other words, in at least one embodiment, the "pressed" surface finish of the composite material can vary between N1 (very fine ground surface) and N8 (smooth machined surface). In various embodiments, the composite material can be capable of maintaining a polished mirror surface after appropriate finishing.

[0113] According to at least one embodiment, the composite material has a flexural strength of about 10 MPa to 25 MPa, with a flexural strength of 12 MPa to 15 MPa being even more preferred.

[0114] According to at least one embodiment, the graphite present in the composite material is a registered graphite, wherein the graphite is registered in a predetermined direction. In some embodiments, the registration of the graphite in such articles is achieved by roll forming and other similar techniques. In one embodiment, the registration of the graphite is the result of the mode or manner in which the 3D print head moves when the article is 3D printed. In one embodiment, the registration of the graphite is the result of the manner in which the granular mixture is extruded through the extrusion head. In one embodiment, the registration of the graphite is achieved by uniaxial pressing or isostatic pressing. In various embodiments, the presence of registered graphite can lead to excellent metal corrosion resistance and mechanical toughness. In some embodiments, the presence of registered graphite further provides a potential way to improve the corrosion resistance of the manufactured article to flux, slag and metal corrosion. In various embodiments, by forming a method of registered graphite, a composite material containing registered graphite can form an article exhibiting excellent corrosion resistance.

[0115] In various embodiments, the composite material further has a non-wetting surface.

[0116] In accordance with at least one embodiment, the composite material is in substantially net shape.

[0117] In some embodiments, carbon black, flake graphite, needle coke, and a binder system provide 100% of the total weight of the granular mixture. In such embodiments, other than carbon black, flake graphite, needle coke, and a binder system, no other components (including the aforementioned "additives") are present in the granular mixture of the present disclosure. In such embodiments, when such a granular mixture is formed into a molded body consisting of the granular mixture, and the molded body is fired to provide a composite material comprising graphite, the resulting composite material has a total carbon content of at least 99%.

[0118] According to at least one embodiment, the composite material has pores larger than 0.005 μm, which are blocked by the antioxidant additive. According to at least one embodiment, the antioxidant additive in the article comprises a first antioxidant additive group and a second antioxidant additive group, the first antioxidant additive group comprising boron carbide, silicon carbide, aluminum zinc phosphate, or any combination thereof, the second stage antioxidant additive group is different from the first antioxidant additive group and comprises zinc phosphate, aluminum phosphate, aluminum zinc phosphate, or any combination thereof.

[0119] Preferably, at least a portion of the composite material is further coated with a coating. In other words, at least a portion of the surface of the composite material is coated with a coating. Advantageously, the coating is at least one selected from the group comprising: boron nitride, silicon carbide, aluminum oxide or aluminum titanate.

[0120] In some embodiments, the composite material is infiltrated with silicone, a selected phosphate solution, or any combination thereof.

[0121] In one embodiment, a composite material comprising graphite is obtained by the method of the invention. According to at least one embodiment, an article is obtained from a composite material as previously detailed. BRIEF DESCRIPTION OF THE DRAWINGS

[0122] Figure 1 is a plot showing the particle size distribution of a granular mixture before firing and the pore size distribution in a part after firing according to the present disclosure. Figure 1As shown in (see the far left, e.g., labeled 'Particle size in graphite mixture'), the particulate mixture has a bimodal particle size distribution, wherein a first group of particles have a particle size diameter of about 50 μm to about 100 μm, and a second group of particles have a particle size diameter of about 110 μm to about 1000 μm. The first group of particles may constitute about 30 volume percent to about 60 volume percent of the total particulate mixture, while the second group of particles may constitute about 20 volume percent to about 40 volume percent of the total particulate mixture (as noted elsewhere in this disclosure, the particle sizes expressed herein are D50 particle sizes, i.e., half of the particles are above the value expressed, and the other half of the particles are below the value expressed). Figure 1 Also shown is the pore size distribution of an exemplary granular mixture after firing.

[0123] Figure 2A and 2B is a SEM (scanning electron microscope) image of a composite structure of graphite according to an embodiment of the present disclosure, which shows that the graphite in the composite structure is registered graphite. Figure 2A and 2B It is an SEM image showing a graphite composite material comprising aligned graphite prepared according to the present disclosure. The use of alignment in graphite is well known in the manufacture of crucibles as molten metal containers. In some embodiments, the alignment of graphite in such articles is achieved by roll forming and other similar techniques. In one embodiment, the alignment of graphite is the result of the mode or manner in which the 3D print head moves when the article is 3D printed. In one embodiment, the alignment of graphite is the result of the manner in which the granular mixture is extruded by the extrusion head. In one embodiment, the alignment of graphite is achieved by uniaxial pressing or isostatic pressing. In various embodiments, the presence of aligned graphite can result in excellent metal corrosion resistance and mechanical toughness. In some embodiments, the presence of aligned graphite further provides a potential way to improve the corrosion resistance of manufactured articles to flux, slag and metal corrosion. In various embodiments, by forming a method of aligned graphite, a composite material comprising aligned graphite can result in the formed article exhibiting excellent corrosion resistance.

[0124] Figure 3 is a SEM image of a composite material according to an embodiment of the present disclosure, wherein clay and aluminum zinc phosphate (Al, Zn phosphate) are located near needle coke. Figure 3 is a SEM image of a composite material according to the present disclosure, the composite material comprising an aluminum zinc phosphate ((Al,Zn)P) antioxidant additive (e.g., added as a first stage antioxidant additive and / or as a second stage antioxidant additive) located near needle coke. The SEM image shows that the addition of the antioxidant additive closes the pores of the composite structure, as shown in FIG. Figure 4 It is worth noting that Figure 4 The pore size distributions of the base composite material S1 according to the present disclosure and the composite materials S2, S3 and S4 containing various additives according to the embodiments of the present disclosure were compared. The base composite material S1 was made of a granular mixture of carbon black, flake graphite, needle coke and a binder system only, while the composite material S2 was made of a granular mixture of carbon black, flake graphite, needle coke, a binder system and (Al, Zn) P, S3 was made of a granular mixture of carbon black, flake graphite, needle coke, a binder system and (Al, Zn) P, which was impregnated with siloxane after firing, and the composite material S4 was made of a granular mixture of carbon black, flake graphite, needle coke and a binder system, which was impregnated with siloxane after firing. Figure 4 The addition of (Al,Zn)P to a granular mixture of carbon black, flake graphite, needle coke, and a binder system closes the pores by forming a glass (compare S1 to S2) or other similar glazing or glaze-like layer, where the density increases from 1.64 g / cm2 of S1 to 1.64 g / cm2 of S2. 3 Change to S2's 1.67 g / cm 3 . Figure 4 It is also shown that siloxane infiltration into a particulate mixture of carbon black, flake graphite, needle coke and a binder system with or without (Al,Zn)P closes all or most of the remaining pores (compare S3 to S2 and S1 to S4), with varying densities.

[0125] Figure 4 is a plot comparing the pore size distribution of a base composite material according to the present disclosure and composite materials including various additives according to embodiments of the present disclosure.

[0126] Figure 5A and 5B is a SEM image of a composite material including a toughening / strength enhancing additive according to an embodiment of the present disclosure. Figure 5A and 5B SEM images of composite materials according to embodiments of the present disclosure are provided, the composite materials comprising a toughening / strength enhancing additive (e.g., carbon fiber bundles). These SEM images show that the toughening / strength enhancing additive is well bonded to the matrix graphite. Moreover, the oxidation package ensures good bonding and siloxane infiltration further enhances bonding. The carbon fiber bundles participate in the fracture process to provide long crack bridging or toughness enhancement.

[0127] Figure 6 is a SEM image of a composite material including a wear / erosion resistant agent according to an embodiment of the present disclosure. Figure 6is an SEM image of a composite material according to an embodiment of the present disclosure, the composite material comprising a wear / erosion resistant agent (e.g., zirconium oxide). The addition of a wear / erosion resistant agent (e.g., zirconium oxide) can react with an antioxidant additive to form an erosion / oxidation resistant zircon (zirconium silicate, ZrSiO4) and / or ZrSi glass.

[0128] Figure 7 is a plot showing Figure 6 Pore ​​size distribution of the composites shown.

[0129] Fig. 8A and 8B is a SEM image of a composite material according to an embodiment of the present disclosure, the composite material comprising a thermal insulation reinforcement; Fig. 8A The thermal insulation enhancing agent is dispersed in the particles of the granular mixture used to provide the composite material, and Figure 8B The thermal insulation enhancing agent is shown to be located between the particles of the granular mixture used to provide the composite material. Fig. 8A The thermal insulation enhancer is shown dispersed in the particles of the granular mixture used to provide the composite material S5, while Figure 8B The thermal insulation enhancing agent is shown to be located between the particles of the granular mixture used to provide the composite material S6.

[0130] Fig. 9 is a plot showing Fig. 8A (S5) and 8B (S6) pore size distribution of the composites shown.

[0131] Fig.10 is a bright bitmap image of a composite material according to an embodiment of the present disclosure, the composite material comprising NiP.

[0132] Fig.11 is a plot showing Fig.10 Pore ​​size distribution of the composites.

[0133] It should be noted that Figure 1 , 4 The pore diameters shown in , 7, 9 and 11 are based on mercury (Hg) intrusion analysis, as described in detail previously.

[0134] Examples

[0135] Example 1:

[0136] In this example, the granular mixture is entirely composed of 88.0 weight percent natural flake graphite, 7.0 weight percent medium molecular weight phenolic resin powder and 5.0 weight percent dibasic ester. Natural flake graphite and phenolic resin are placed in a single hopper in batches and then added to a blender without adding dibasic ester. Dry components are added to the blender and dry blended for about 2 minutes. After dry blending, dibasic ester components are added and the strength of the blender is increased. The mixing process lasts for about 30-45 minutes until the granular mixture is fully granulated. After measurement, the loose packing density of the granular mixture is about 0.51g / cm 3 After cooling to room temperature, the granular mixture was isostatically pressed at about 5,000 psi. The pressed body had a density of 1.6 g / cm 3 The green density of the molten steel was 0.13 W and the green strength was very low. Adding phenolic resin and DBE resulted in a non-flowing powder that could not be easily formed into a molded body. Although the molded body was cured at 200°C, this only resulted in further weakening of the molded body and eventual fracture.

[0137] Example 2:

[0138] In this example, the granular mixture contains 76.0 weight percent natural flake graphite, 7.5 weight percent carbon black, and 3.0 weight percent needle coke, 7.5 weight percent medium molecular weight phenolic resin powder, and 5.0 weight percent dibasic ester. The dry components are placed in a single hopper in batches and then added to the blender without adding dibasic ester. The dry components are added to the blender and dry blended for about 2 minutes. After dry blending, dibasic ester is added and the strength of the blender is increased. The mixing process is carried out for about 30-45 minutes until the granular mixture is fully granulated. After measurement, the loose packing density of the mixture is about 0.65g / cm 3 After cooling to room temperature, the mixture was exposed to isostatic pressing at about 5,000 psi. The pressed body had a density of 1.7 g / cm 3 After pressing, the molded body was cured at 200°C. The curing process resulted in crosslinking of the resin, which further increased the handling strength. The cured molded body was exposed to a final firing cycle at 1200°C for 4 hours. The resulting article included a pore profile as disclosed in the present disclosure. The surface roughness and profile were measured and as described in the previous examples and figures, especially Figure 2A and 2B As disclosed in.

[0139] Example 3:

[0140] This example was carried out according to the same process as Example 2, except that the pressed molded body was infiltrated with a siloxane and / or phosphate solution after curing at 200°C and fired once at 1200°C. The resulting composite material (article) exhibited Figure 4 Pore ​​size distribution shown.

[0141] Example 4:

[0142] This example was carried out according to the same process as Example 2, except that the fired article was impregnated with a siloxane and / or phosphate solution. After drying, the impregnated article was fired a second time in a carbon-containing environment at 1000°C. The resulting composite material (article) exhibited Figure 4 The pore size distribution is shown. Figure 3 , which shows an SEM image of a composite material according to this example, in which clay and aluminum zinc phosphate are located near needle coke.

[0143] The applicant has noted that the impregnation treatment helps to prevent oxidation of the carbon fibres during field application and also results in the closure of many of the coarser pores and therefore in an article with increased density.

[0144] Example 5:

[0145] In this example, the granular mixture contains a combination of 76.0 weight percent natural flake graphite, 7.5 weight percent carbon black, 3.0 weight percent needle coke, and 13.0 weight percent liquid medium molecular weight phenolic resin mixture. The liquid phenolic resin is prepared by premixing the phenolic resin with a dibasic ester at a ratio of 70:30 or with ethylene glycol at a ratio of 55:45. The dry components are placed in batches in a single hopper and then added to a mixer and dry blended in the mixer for about 2 minutes. After dry blending, the resin is added to the mixer and the strength of the mixer is increased. The mixing process is carried out for about 30-45 minutes until the granular mixture is fully granulated. It has been measured that the loose packing density of the granular mixture is about 0.65g / cm 3 After cooling to room temperature, the mixture was exposed to isostatic pressing at about 5,000 psi. The pressed body had a density of 1.7 g / cm 3 The green density of the molded body and the green strength for easy handling. After pressing, the molded body is transferred to a kiln and cured at 200°C. The curing process causes the resin to crosslink, which further increases the handling strength. The cured molded body is exposed to a final firing cycle at 1200°C for 4 hours. The resulting article includes a hole profile as disclosed in the present disclosure. The surface roughness and profile are measured and as disclosed in the previous examples and figures.

[0146] Example 6:

[0147] This example was conducted according to the same process as Example 5, except that the pressed molded body was infiltrated with a siloxane and / or phosphate solution after curing at 200° C. and fired once at 1200° C. The resulting article included a hole profile as disclosed in the present disclosure. The surface roughness and profile were measured and as disclosed in this patent application.

[0148] Example 7:

[0149] This example was carried out according to the same process as Example 5, except that the fired article was impregnated with a siloxane and / or phosphate solution. After drying, the impregnated article was fired a second time in a carbon-containing environment at 1000° C. The applicant noted that the impregnation treatment helped to prevent oxidation of the carbon fibers during field application and also resulted in the closure of many coarser pores and, therefore, an article with increased density.

[0150] Example 8:

[0151] In this example, the granular mixture contains 70.0 weight percent natural flake graphite, 6.0 weight percent carbon black, and 2.0 weight percent needle coke, 5.0 weight percent boron carbide, 3.3 weight percent silicon carbide, 7.0 weight percent medium molecular weight phenolic resin powder, and 5.0 weight percent dibasic ester. In this example, 1.7 weight percent of zirconium oxide powder is added to the dry components. The dry components are placed in a single hopper in batches and then added to the blender without adding dibasic ester. The dry components are added to the blender and dry blended for about 2 minutes. After dry blending, dibasic ester is added to the blender and the strength of the blender is increased. The mixing process is carried out for about 30-45 minutes until the granular mixture is fully granulated. After measurement, the loose packing density of the mixture is about 0.68g / cm 3 After cooling to room temperature, the granulated mixture was isostatically pressed at about 5,000 psi. The pressed body had a density of 1.75 g / cm 3 green density as well as green strength for easy handling. After pressing, the molded bodies are cured at 200°C. The curing process causes the resin to crosslink, which further increases the handling strength. The cured molded bodies are exposed to a final firing cycle at 1200°C for 4 hours. Figure 6 , which is a SEM image of a composite material containing a wear / corrosion resistant agent according to this example. The resulting article comprises Figure 7 The inventors have discovered that zirconium oxide powder provides enhanced wear resistance to the resulting article.

[0152] Example 9:

[0153] This example was conducted according to the same process as Example 8, except that the pressed molded body was infiltrated with a siloxane and / or phosphate solution after curing at 200° C. and fired once at 1200° C. The resulting article included a pore profile as disclosed in the present disclosure. The surface roughness and profile were measured and as disclosed in the previous examples and figures.

[0154] Example 10:

[0155] This example was carried out according to the same process as Example 8, and the fired article was infiltrated with a siloxane and / or phosphate solution. After drying, the infiltrated article was fired a second time in a carbon-containing environment at 1000°C.

[0156] The applicant has noted that the impregnation treatment helps to prevent oxidation of the carbon fibres during field application and also results in the closure of many of the coarser pores and therefore in an article with increased density.

[0157] Example 11:

[0158] In this example, the granular mixture contains 70.0 weight percent natural flake graphite, 6.0 weight percent carbon black, and 2.0 weight percent needle coke, 5.0 weight percent boron carbide, 3.3 weight percent silicon carbide, 7.0 weight percent medium molecular weight phenolic resin powder, and 5.0 weight percent dibasic ester. The dry components are placed in batches in a single hopper and then added to the mixer without adding dibasic ester. The dry components are added to the mixer and dry blended for about 2 minutes. After dry blending, the dibasic ester is added to the mixer and the strength of the mixer is increased. The mixing process is carried out for about 30-45 minutes until the granular mixture is fully granulated. Add 1.7wt.% of insulating aluminum silicate fiber and continue mixing for another 1 or 2 minutes. It has been measured that the loose packing density of the granular mixture is about 0.63g / cm 3 After cooling to room temperature, the granular mixture was isostatically pressed at about 5,000 psi. The pressed body had a density of 1.72 g / cm 3 green density as well as green strength for easy handling. After pressing, the molded bodies are cured at 200°C. The curing process causes the phenolic resin to crosslink, which further increases the handling strength. The cured molded bodies are exposed to a final firing cycle at 1200°C for 4 hours. Fig. 8A and 8B , which shows a SEM image of the composite material obtained according to this example; Fig. 8A The thermal insulation enhancing agent is dispersed in the particles of the granular mixture used to provide the composite material, and Figure 8B The thermal insulation enhancing agent is shown to be located between the particles of the granular mixture used to provide the composite material. The pore size distribution of the composite material is shown in Fig. 9 middle.

[0159] Example 12:

[0160] This example was conducted according to the same process as Example 11, except that the pressed molded body was infiltrated with a siloxane and / or phosphate solution after curing at 200° C. and fired once at 1200° C. The resulting article included a pore profile as disclosed in the present disclosure. The surface roughness and profile were measured and as disclosed in the previous examples and figures.

[0161] Example 13:

[0162] This example was carried out according to the same process as Example 11, except that the fired article was infiltrated with a siloxane and / or phosphate solution. After drying, the infiltrated article was fired a second time in a carbon-containing environment at 1000°C.

[0163] The Applicant has observed that the infiltration treatment causes the closure of a large part of the coarser pores and therefore leads to a product with increased density.

[0164] Example 14:

[0165] In this example, the granular mixture contains 70.0 weight percent natural flake graphite, 6.0 weight percent carbon black, and 2.0 weight percent needle coke, 5.0 weight percent boron carbide, 3.5 weight percent silicon carbide, 7.0 weight percent medium molecular weight phenolic resin powder, and 5.0 weight percent dibasic ester. The dry components are placed in batches in a single hopper and then added to the mixer without adding dibasic ester. The dry components are added to the mixer and dry blended for about 2 minutes. After dry blending, the dibasic ester is added to the mixer and increases the strength of the mixer. The mixing process is carried out for about 30-45 minutes until the granular mixture is fully granulated. Add 1.5wt.% of chopped carbon fiber bundles with a length of 6mm and a width of 3mm and continue mixing for another 1 to 2 minutes. It has been measured that the loose packing density of the granular mixture is about 0.63g / cm 3 After cooling to room temperature, the granular mixture was isostatically pressed at about 5,000 psi. The pressed body had a density of 1.72 g / cm 3 green density as well as green strength for easy handling. After pressing, the molded bodies are cured at 200°C. The curing process causes the phenolic resin to crosslink, which further increases the handling strength. The cured molded bodies are exposed to a final firing cycle at 1200°C for 4 hours. Figure 5A and 5B , which shows an SEM image of a composite material including a toughening / strength enhancing additive according to an embodiment of the present disclosure.

[0166] The applicant observed that both the strength and toughness of the present article were increased compared to graphite articles not containing carbon fibers. The carbon fiber bundles were found to be strongly bonded to the graphite and participate in the fracture mechanism. The surface roughness and profile were measured and as disclosed in the previous examples and figures.

[0167] Example 15:

[0168] This example was carried out according to the same process as Example 14, except that the pressed molded body was infiltrated with a siloxane and / or phosphate solution after curing at 200°C and fired once at 1200°C.

[0169] Example 16:

[0170] This example was carried out according to the same process as Example 14, except that the fired article was infiltrated with a siloxane and / or phosphate solution. After drying, the article was fired a second time in a carbon-containing environment at 1000°C.

[0171] The Applicant has noted that the infiltration treatment is very important to prevent oxidation of the carbon fibers during field application. As reported in previous examples, the infiltration treatment also causes the closure of most of the coarser pores and thus results in an article with increased density.

[0172] Although the present disclosure has been particularly shown and described with respect to the preferred embodiments of the present disclosure, it will be understood by those skilled in the art that the foregoing and other changes in form and detail may be made without departing from the spirit and scope of the present disclosure. Therefore, it is not intended that the present disclosure be limited to the exact forms and details described and illustrated, but rather fall within the scope of the appended claims.

Claims

1. A method of forming an article comprising a composite material containing graphite, wherein the article is suitable for containing or processing molten metal, the method comprising the steps of: (a) forming at least one pelletized mixture by mixing at least carbon black, flake graphite, needle coke and at least one resin, wherein the at least one resin has a flow distance of 20 mm to 150 mm as measured by ISO 8619:2003; (b) shaping the at least one particulate mixture into at least one shaped body; and (c) firing the at least one shaped body.

2. The method of claim 1, wherein: Relative to the total weight of the granulated mixture: The carbon black is present in the particulate mixture in an amount of about 5 weight percent to about 10 weight percent, preferably in an amount of about 5 weight percent to about 8 weight percent, The flake graphite is present in the particulate mixture in an amount of about 65 weight percent to about 85 weight percent, preferably about 75 weight percent to about 80 weight percent, The needle coke is present in the particulate mixture in an amount of about 1 weight percent to about 5 weight percent, preferably about 2 weight percent to about 4 weight percent, and The resin is present in the granular mixture in an amount of about 2 weight percent to about 10 weight percent, preferably about 6 weight percent to about 8 weight percent.

3. The method according to claim 1 or 2, wherein: At least one solvent is added to the at least one resin to form at least one binder system consisting of the at least one resin and the at least one solvent.

4. The method of claim 3, wherein: The at least one solvent is present in the granular mixture in an amount of about 1 weight percent to about 5 weight percent, preferably about 3 weight percent to about 4 weight percent, relative to the total weight of the granular mixture.

5. The method according to any one of claims 1 to 4, wherein: The at least carbon black, the flake graphite, the needle coke and the at least one resin provide 100% of the total weight of the particulate mixture.

6. The method according to any one of claims 1 to 5, wherein: The at least one granular mixture further comprises about 5 weight percent to about 15 weight percent of at least one antioxidant additive relative to the total weight of the granular mixture, wherein optionally, the at least one antioxidant additive comprises boron carbide, silicon carbide, aluminum zinc phosphate, or any combination thereof.

7. The method according to any one of claims 1 to 6, wherein: The at least one granular mixture further comprises from about 1 weight percent to about 5 weight percent of at least one toughening / strength enhancing additive relative to the total weight of the granular mixture, wherein optionally, the at least one toughening / strength enhancing additive comprises carbon fibers, chopped carbon fiber bundles, basalt bundles, aluminum silicate fibers, chopped steel fibers, or any combination thereof.

8. The method according to any one of claims 1 to 7, wherein: The granular mixture further comprises about 1 weight percent to about 10 weight percent of at least one wear / erosion resistant agent relative to the total weight of the granular mixture, wherein optionally, the at least one wear / erosion resistant agent comprises a metal oxide, a metal nitride, a metal boride, or any combination thereof.

9. The method according to any one of claims 1 to 8, wherein: The at least one granular mixture further comprises from about 1 weight percent to about 5 weight percent of an insulation enhancer relative to the total weight of the granular mixture, and wherein optionally, the at least one insulation enhancer comprises colloidal silica pellets, preferably aluminum colloidal silicate pellets, a mixture of fibers, preferably sodium and chopped silica fibers, or a mixture thereof.

10. The method according to any one of claims 1 to 9, wherein: At least a portion of the composite material is infiltrated with siloxane, a selected phosphate solution, or any combination thereof, either before or after the firing step.

11. The method according to any one of claims 10, wherein: The resin is a phenolic resin, wherein optionally, the phenolic resin is a liquid phenolic resin.

12. An article comprising a composite material containing graphite, wherein the composite material has a total pore volume and a pore size distribution measured according to ASTM C830-00 (2016) standard, wherein at least 95% of the total pore volume is contained in pores with a diameter less than 1 μm, and at least 40% of the pore volume of pores with a diameter less than 1 μm is contained in pores with a diameter less than 0.1 μm.

13. The article of claim 12, wherein: The composite material has a thickness of about 1.6 g / cm 3 to about 1.92g / cm 3 density.

14. The article of claim 12 or 13, wherein: The composite material has a graphite content of 65% or more.

15. The article of any one of claims 12 to 14, wherein The composite material has a surface roughness R between 3.2 μm and 0.025 μm. a , where the surface roughness R a It is measured based on ISO 1302:1992 standard.

16. The article of any one of claims 12 to 15, wherein At least a portion of the composite material is further coated with a coating, wherein the coating is preferably at least one coating selected from the group comprising: boron nitride, silicon carbide, aluminum oxide or aluminum titanate.

17. The article of any one of claims 12 to 16, wherein The article is a crucible consisting of a plurality of crucible rings which are evenly stacked on top of each other in order to provide the crucible.

18. An article comprising a composite material comprising graphite obtained by the method according to any one of claims 1 to 11.

19. The article of claim 18, wherein: The composite material has a total pore volume and pore size distribution measured according to ASTM C830-00 (2016) standard, wherein at least 95% of the total pore volume is contained in pores with a diameter less than 1 μm, and at least 40% of the pore volume of pores with a diameter less than 1 μm is contained in pores with a diameter less than 0.1 μm.

20. The article of claim 18 or claim 19, wherein: At least a portion of the composite material is further coated with a coating, wherein the coating is preferably at least one coating selected from the group comprising: boron nitride, silicon carbide, aluminum oxide or aluminum titanate.

21. The article of any one of claims 18 to 20, wherein The article is a crucible consisting of a plurality of crucible rings which are evenly stacked on top of each other in order to provide the crucible.

Citation Information

Patent Citations

  • Plastic component comprising carbon filler

    CN108290795A

  • Preparation method of carbon contact strip of collector shoe, and carbon contact strip of collector shoe

    CN109867522A

  • Carbon fibre-reinforced carbon heating element prodn. - involves chemical gas phase infiltration with pyrolytic carbon

    DE3922539A1

  • Insulating refractory material

    US6559082B1