Coated blood flow guide stent and preparation method

By forming a composite coating structure with hydroxyl-rich, organic acid or polymer and titanium dioxide layer on the blood flow-guided stent, the problem of insufficient anticoagulation effect and adhesion strength in the prior art is solved, and the anticoagulation of the stent is significantly improved Performance and adhesion strength enhance biosafety.

CN118873757APending Publication Date: 2024-11-01JIANGSU NOWYON MEDICAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411072891.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The anticoagulant effect and adhesion strength of existing blood flow-guided stent coatings cannot fully meet clinical needs, resulting in an increased risk of thrombotic events.

Method used

Using a coating structure, including a hydroxyl-rich layer, an organic acid layer or polymer layer and a titanium dioxide layer on a metal bracket, it is formed by NaOH solution treatment, an organic acid or polymer solution water bath and a titanium dioxide solution water bath, etc., combined with ultraviolet light Irradiation improves adhesion strength and anticoagulation effect.

Benefits of technology

It significantly improves the anticoagulation performance and adhesion strength of the scaffold surface, reduces the adsorption between proteins and platelets, promotes vascular endothelialization, enhances biocompatibility and corrosion resistance, reduces the release of metal ions, and improves the biologic Security.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118873757A_ABST
    Figure CN118873757A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of medical instruments, in particular to a coated blood flow guide stent and a preparation method. The invention discloses a coating blood flow guide stent and a preparation method thereof. The coating blood flow guide stent comprises a metal stent and a titanium dioxide layer covering the surface of the metal stent, the metal support is covered with a hydroxyl-rich base layer, the hydroxyl-rich base layer is covered with an organic acid layer or / and a polymer layer, and the organic acid layer or / and the polymer layer is covered with a titanium dioxide layer. The technical problem that in the prior art, the anticoagulation effect of a blood flow guide stent coating and the adhesion strength of the coating and a stent cannot completely meet the clinical effect is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical devices, and in particular to a coated blood flow guiding stent and a preparation method thereof. Background Art

[0002] Intracranial aneurysms are caused by damage to the arterial wall and aging due to cerebral arterial wall dysplasia, postnatal injury, atherosclerosis, etc., which leads to abnormal expansion of intracranial blood vessels and aneurysmal protrusions of the wall. In the general population, the prevalence of intracranial aneurysms is 2% to 3%, and it can occur at any age, but its peak age is 40 to 60 years old. Aneurysms in this age range account for about 60% of all intracranial aneurysms, and most of them occur in women. Intracranial aneurysms are insidious, and once ruptured, the disability and mortality rates are high, and the mortality rate can be as high as 50%.

[0003] Common treatments for intracranial aneurysms include open surgery for aneurysm clipping, endovascular intervention for aneurysm embolization, and vascular reconstruction. With the reports of clinical studies on the efficacy of blood flow-directed stents in curing aneurysms, the use of blood flow-directed stents to achieve reconstruction of the parent artery has become a hot topic in current treatment.

[0004] The high metal coverage of blood flow-directed stents increases the cure rate of intracranial aneurysms, but also increases the risk of thrombotic events. Therefore, the surface coating modification of blood flow-directed stents improves the anticoagulant properties of the stent surface and reduces the probability of acute thrombosis, which is gradually gaining attention as a supplement to antiplatelet aggregation therapy.

[0005] For example, Chinese patent document CN115836896A uses electrografting technology to coat a coating containing a polymer on the surface of a stent. For example, Chinese patent document CN113262331A uses a chemical conversion method to treat a nickel-titanium alloy dense mesh stent to obtain a titanium dioxide base layer on the surface of the stent, and grafts organic small molecules such as ferulic acid on the surface of the titanium dioxide base layer to form an organic small molecule functional coating with nanoscale anticoagulant function. However, the anticoagulant effect of the current blood flow guiding stent coating and the adhesion strength of the coating and the stent cannot fully meet the clinical effect, and there is still a lot of room for improvement. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and to provide a coated blood flow guiding stent and a preparation method, which aims to solve the technical problems in the prior art that the anticoagulant effect of the blood flow guiding stent coating and the adhesion strength between the coating and the stent cannot fully meet the clinical effect.

[0007] To achieve the above objectives, the present invention proposes a coated blood flow guiding stent, comprising a metal stent and a titanium dioxide layer covering the surface of the metal stent; the metal stent is covered with a hydroxyl-rich layer, the hydroxyl-rich layer is covered with an organic acid layer and / or a polymer layer, and the organic acid layer and / or the polymer layer is covered with a titanium dioxide layer.

[0008] Preferably, the metal stent composition includes one or more of cobalt-chromium alloy, platinum-tungsten alloy, nickel-titanium alloy, magnesium alloy, stainless steel, and titanium alloy.

[0009] Preferably, the components of the organic acid layer include one or more of phytic acid and tannic acid.

[0010] Preferably, the components of the polymer layer include one or more of polydopamine, chitosan, heparin, phosphorylcholine, and polyurethane.

[0011] To achieve the above object, the present invention proposes a method for preparing a coated blood flow guiding stent, which is used to prepare the above-mentioned coated blood flow guiding stent, comprising the following steps: S1: Clean the metal bracket, dry it after cleaning and set it aside; S2: preparing a NaOH solution, placing the metal stent in a water bath in the NaOH solution, rinsing the stent with deionized water after the water bath, and drying to obtain a metal stent sample with a hydroxyl-rich layer; S3: placing the metal stent sample with a hydroxyl-rich surface treated in step S2 into an organic acid or polymer solution for a water bath, and rinsing the stent with deionized water and drying it after the water bath to obtain a metal stent sample covered with an organic acid layer or a polymer layer; S4: preparing titanium dioxide solution; S5: placing the metal stent treated in step S3 into the titanium dioxide solution in step S4 for a water bath. After the water bath, rinse the stent with deionized water and dry it to obtain a metal stent sample covered with a titanium dioxide layer.

[0012] Preferably, the cleaning process in S1 is ultrasonic cleaning in acetone, anhydrous ethanol and deionized water in sequence; the concentration of the NaOH solution in S2 is 3 mol / L, the water bath temperature is 60° C., and the water bath time is 12 h.

[0013] Preferably, when preparing the metal stent sample with the organic acid layer in S3, a phytic acid solution with a concentration of 5 mg / ml is prepared, the pH value of the phytic acid solution is adjusted to 5 using NaOH, and the stent sample with a hydroxyl-rich surface is placed in a water bath in the phytic acid solution at 50° C. for 4 hours.

[0014] Preferably, when preparing the metal stent sample with an organic acid layer in S3, a 2 mg / ml tannic acid solution is prepared, wherein the concentration of the selected Tris-HCl solution is 2 mg / ml, and the pH value is adjusted to 10 by NaOH, and the stent sample with a hydroxyl-rich surface is placed in the solution and placed in a water bath at 30°C for 2 hours.

[0015] Preferably, when preparing the metal stent sample of the polymer layer in S3, a 2 mg / ml dopamine hydrochloride solution is prepared, wherein the selected tris-base solution concentration is 15 mol / mL and the pH value is 8.5, and the stent sample with a hydroxyl-rich surface is placed in the solution and placed in a water bath at 37°C for 6 hours.

[0016] Preferably, the preparation process in S4 is: prepare an ammonium fluorotitanate solution with a concentration of 0.1 mol / L, prepare a boric acid solution with a concentration of 0.35 mol / L, place the prepared ammonium fluorotitanate solution and the boric acid solution in a water bath at 60°C for 12 hours, mix the prepared ammonium fluorotitanate solution and the boric acid solution in a volume ratio of 1:1, and use hydrofluoric acid to adjust the pH value of the mixed solution to 2.8 to obtain a titanium dioxide solution.

[0017] Preferably, the water bath temperature in S5 is 50° C., the water bath time is 1 hour, and the stent sample is irradiated with ultraviolet light with a wavelength of 254 nm during the water bath.

[0018] Compared with the prior art, the coated blood flow guiding stent and the preparation method thereof provided by the present invention have the following beneficial effects: 1. Titanium dioxide coating has good biocompatibility and hydrophilicity. Coating on the surface of the stent can reduce the adsorption of proteins and platelets, improve the anticoagulant properties of the stent, and inhibit the formation of thrombus. Titanium dioxide coating is brittle. When directly coated on the surface of the metal substrate, it adheres by covalent bonds. Its adhesion strength cannot meet the needs of clinical use. The phytic acid layer can be firmly connected with the hydroxyl groups on the hydroxyl-rich surface (reaction 1). The chelation of titanium dioxide with the hydroxyl groups on the surface of the phytic acid layer (reaction 2) can improve its adhesion strength. At the same time, the grid structure brought by the organic acid layer can effectively promote the endothelialization of blood vessels as a stent for endothelial cells to crawl. Ultraviolet light irradiation causes titanium dioxide to produce photoelectrons and holes, improves the activity of titanium dioxide, promotes the chelation of phytic acid and titanium dioxide, and promotes the uniform coating of titanium dioxide coating to obtain high-quality titanium dioxide coating. Titanium dioxide coating has good corrosion resistance and does not release toxic ions in the blood. The combination of hydroxyl-rich surface, phytic acid layer and titanium dioxide coating can effectively prevent the release of metal ions in the substrate and improve the biosafety of the stent. It can effectively improve the anticoagulant effect on the surface of the blood flow guiding stent and increase the adhesion strength between the coating and the stent.

[0019] 2. Polydopamine can be firmly connected to the metal substrate with a hydroxyl-rich surface under the combined action of covalent bonds and non-covalent bonds formed by its catechol functional groups and the substrate. The amino, phenolic hydroxyl and other functional groups of polydopamine chelate titanium dioxide in a similar manner to reaction 2, thereby improving the adhesion strength of titanium dioxide. The grid structure brought by the polymer layer can effectively promote vascular endothelialization as a scaffold for endothelial cells to crawl on. Polydopamine (PDA) has a structure and strong adhesion similar to that of adhesion proteins. The PDA film can be quickly formed on the surface of the substrate in an alkaline solution. Due to the hydrophilic hydroxyl and amino groups of PDA, the hydrophilicity and chemical versatility of the substrate are improved. The PDA layer can be used as an intermediate to anchor the functional molecules on the surface through chemical bonds (through Michael addition or Schiff base reaction) or other physical bonds (hydrogen bonds or van der Waals forces).

[0020] The features and advantages of the present invention will be described in detail through embodiments in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the morphology of the sample in Example 1 before entering the 0.027-inch sheath tube (observed at 100,000 times magnification).

[0022] Figure 2 This is the morphology of the sample in control group 1 before entering the 0.027-inch sheath (observed at 100,000x magnification).

[0023] Figure 3 This is the morphology of the sample in Example 1 after entering and exiting the 0.027-inch sheath tube five times (observed at 100,000 times magnification).

[0024] Figure 4 This is the morphology of the sample in control group 1 after entering and exiting the 0.027-inch sheath tube five times (observed at 100,000x magnification).

[0025] Figure 5 This is the morphology of the sample in Example 1 before entering the 0.027-inch sheath tube (observed at 50,000 times magnification). DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0027] In the description of the present invention, it should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.

[0028] In the description of the present invention, it should be noted that the terms "center", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the invention product is usually placed when in use, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third" and the like are only used to distinguish descriptions, and cannot be understood as indicating or implying relative importance. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.

[0029] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0030] An embodiment of the present invention provides a coated blood flow guiding stent, comprising a metal stent and a titanium dioxide layer coated on the surface of the metal stent; the metal stent is coated with a hydroxyl-rich layer, the hydroxyl-rich layer is coated with an organic acid layer or / and a polymer layer, and the organic acid layer or / and the polymer layer is coated with a titanium dioxide layer. The components of the organic acid layer include one or more of phytic acid and tannic acid. The organic acid layer is preferably phytic acid. The components of the polymer layer include one or more of polydopamine, chitosan, heparin, phosphorylcholine, and polyurethane. The component of the polymer layer is preferably polydopamine. The titanium dioxide coating exhibits brittleness. When directly coated on the surface of a metal substrate, it adheres by covalent bonds, and its adhesion strength cannot meet the requirements of clinical use. The phytic acid layer (or polymer) can be firmly connected to the hydroxyl groups on the hydroxyl-rich surface (reaction 1). Since the molecular structure of phytic acid is complex and the reaction may involve multiple steps and intermediates, the following reaction formula is only a schematic expression. The chemical formula of reaction 1 is: The chelation of titanium dioxide with the hydroxyl groups on the surface of the phytic acid layer (reaction 2) can improve its adhesion strength. The chemical formula of reaction 2 is: . At the same time, the grid structure brought by the phytic acid layer (or polymer) can effectively promote the endothelialization of blood vessels as a stent for endothelial cells to crawl. Ultraviolet light irradiation causes titanium dioxide to produce photoelectrons and holes, which increases the activity of titanium dioxide, promotes the chelation of phytic acid and titanium dioxide, and promotes the uniform coating of the titanium dioxide coating to obtain a high-quality titanium dioxide coating. The titanium dioxide coating has good corrosion resistance and will not release toxic ions in the blood. The combination of hydroxyl-rich surface, phytic acid layer and titanium dioxide coating can effectively prevent the release of metal ions in the substrate and improve the biosafety of the stent. The titanium dioxide coating has good biocompatibility and hydrophilicity. Coating it on the surface of the stent can reduce the adsorption of proteins and platelets, improve the anti-coagulation properties of the stent, and inhibit the formation of thrombus.

[0031] In an optional embodiment, the metal stent composition includes one or more of cobalt-chromium alloy, platinum-tungsten alloy, nickel-titanium alloy, magnesium alloy, stainless steel, and titanium alloy. The metal stents in the following embodiments are all made of cobalt-chromium alloy. Example 1

[0032] The coating layer of the metal stent is a hydroxyl-rich surface, phytic acid and titanium dioxide coating. The metal stent is a cobalt-chromium alloy, and the specific preparation method is as follows: Cleaning of stains: ultrasonically clean the metal bracket in acetone, anhydrous ethanol, and deionized water in order to remove impurities such as grease and fiber on the surface of the bracket. After cleaning, dry the bracket for later use. Acetone cleans organic pollutants, and anhydrous ethanol cleans inorganic pollutants. When both pollutants are involved, organic pollutants are generally cleaned first by default. Deionized water cleaning is placed last to clean the cleaning liquid of the first two steps. The container used is a polytetrafluoroethylene container or a beaker. The experimental containers required below are these two or other containers that will not react with the products contained.

[0033] Obtain a scaffold sample with a hydroxyl-rich surface: prepare a NaOH solution with a concentration of 3 mol / L (the concentration of the NaOH solution can be selected from 0.01 mol / L to 10 mol / L, preferably 3 mol / L), place the scaffold in a 60°C (temperature can be selected from 20°C to 80°C, preferably 60°C) NaOH solution in a water bath for 12 hours (water bath time can be selected from 0-72h, preferably 12h), rinse the scaffold with deionized water after the water bath and dry it to obtain a scaffold sample with a hydroxyl-rich surface.

[0034] Obtain a stent sample coated with a phytic acid layer on a hydroxyl-rich surface: prepare a phytic acid solution with a concentration of 5 mg / ml (the phytic acid solution can be selected from 0.01 mg / ml to 10 mg / ml, preferably 5 mg / ml), use NaOH to adjust the pH value of the phytic acid solution to 5 (the pH value is maintained at 2-7, preferably 5), place the stent sample with a hydroxyl-rich surface in a phytic acid solution at 50°C (the temperature can be selected from 20°C to 80°C, preferably 60°C) for 4 hours (the water bath time can be selected from 0-72h, preferably 4h), rinse the stent with deionized water after the water bath ends and dry it to obtain a stent sample coated with a phytic acid layer on the hydroxyl-rich surface.

[0035] Preparation of titanium dioxide solution: prepare an ammonium fluorotitanate solution with a concentration of 0.025 mol / L (0.005-0.35 mol / L can be selected, preferably 0.025), prepare a boric acid solution with a concentration of 0.075 mol / L (0.005-0.5 mol / L can be selected, preferably 0.075 mol / L), and place the prepared ammonium fluorotitanate solution and boric acid solution in a water bath at 60°C (the temperature can be selected from 20°C to 80°C, preferably 60°C) for 6 hours (the water bath time can be selected from 0-72h, preferably 4h). Mix the ammonium fluorotitanate solution and the boric acid solution after the water bath in a volume ratio of 1:1, and use hydrofluoric acid to adjust the pH value of the mixed solution to 2.8. (In the process of preparing titanium dioxide from ammonium fluorotitanate and boric acid, the chemical equation is relatively complex, and the following is explained by the key equation. Ammonium fluorotitanate will undergo a hydrolysis reaction in an aqueous solution to generate a hydroxyl complex of hydrofluoric acid and titanium. This process can be expressed as: . The pH value and corresponding temperature need to be controlled during the preparation process).

[0036] Obtain the final stent sample with a hydroxyl-rich surface, phytic acid and titanium dioxide coating: place the stent sample coated with a phytic acid layer on the hydroxyl-rich surface in a water bath at 50°C (the temperature can be selected from 20-80°C, preferably 50°C) for 30 minutes (the water bath time can be selected from 0-24h), and irradiate the stent with ultraviolet light with a wavelength of 254nm during the water bath. After the water bath, rinse the stent with deionized water and dry it to obtain the final stent sample with a hydroxyl-rich surface, phytic acid and titanium dioxide coating. Example 2

[0037] The coating layer of the metal stent is a hydroxyl-rich surface, polydopamine and titanium dioxide coating. The specific preparation method is as follows: The metal stent was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water in sequence. After cleaning, the stent was dried for later use.

[0038] A NaOH solution with a concentration of 3 mol / L was prepared, and the stent was placed in a water bath in the NaOH solution at 60° C. for 12 hours. After the water bath, the stent was rinsed with deionized water and dried to obtain a stent sample with a hydroxyl-rich surface.

[0039] A 2 mg / ml dopamine hydrochloride solution was prepared, wherein the concentration of the tris-base solution was 15 mol / mL and the pH value was 8.5. A stent sample having a hydroxyl-rich surface was placed in the solution and placed in a water bath at 37°C for 4 hours. After the water bath, the stent was rinsed with deionized water and dried to obtain a stent sample coated with a polydopamine layer on the hydroxyl-rich surface.

[0040] An ammonium fluorotitanate solution with a concentration of 0.025 mol / L was prepared, and a boric acid solution with a concentration of 0.075 mol / L was prepared. The prepared ammonium fluorotitanate solution and the boric acid solution were placed in a water bath at 60° C. for 6 hours.

[0041] The ammonium fluorotitanate solution and the boric acid solution after the water bath are prepared are mixed in a volume ratio of 1:1, and the pH value of the mixed solution is adjusted to 2.8 with hydrofluoric acid. The stent sample coated with a polydopamine layer on the hydroxyl-rich surface is placed in a water bath at 50°C for 0.5 hours, and the stent is irradiated with ultraviolet light with a wavelength of 254nm during the water bath. After the water bath, the stent is rinsed with deionized water and dried to obtain the final stent sample with a hydroxyl-rich surface, polydopamine and titanium dioxide coating. Example 3

[0042] The coating layer of the metal stent is a hydroxyl-rich surface, tannic acid and titanium dioxide coating. The specific preparation method is as follows: The metal stent was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water in sequence. After cleaning, the stent was dried for later use.

[0043] A NaOH solution with a concentration of 3 mol / L was prepared, and the stent was placed in a water bath in the NaOH solution at 60° C. for 12 hours. After the water bath, the stent was rinsed with deionized water and dried to obtain a stent sample with a hydroxyl-rich surface.

[0044] A 2 mg / ml tannic acid solution was prepared, wherein the concentration of the selected Tris-HCl solution was 2 mg / ml, and the pH value was adjusted to 10 by NaOH. A stent sample having a hydroxyl-rich surface was placed in the solution and placed in a water bath at 50° C. for 4 hours. After the water bath, the stent was rinsed with deionized water and dried to obtain a stent sample coated with a tannic acid layer on the hydroxyl-rich surface.

[0045] An ammonium fluorotitanate solution with a concentration of 0.025 mol / L was prepared, and a boric acid solution with a concentration of 0.075 mol / L was prepared. The prepared ammonium fluorotitanate solution and the boric acid solution were placed in a water bath at 60° C. for 6 hours.

[0046] The ammonium fluorotitanate solution and the boric acid solution after the water bath are prepared are mixed in a volume ratio of 1:1, and the pH value of the mixed solution is adjusted to 2.8 with hydrofluoric acid. The stent sample coated with a polydopamine layer on the hydroxyl-rich surface is placed in a water bath at 50°C for 0.5 hours. During the water bath, the stent is irradiated with ultraviolet light with a wavelength of 254nm. After the water bath, the stent is rinsed with deionized water and dried to obtain the final stent sample with a hydroxyl-rich surface, tannic acid and titanium dioxide coating. Example 4

[0047] The coating layer of the metal stent is a hydroxyl-rich surface, phytic acid and titanium dioxide coating. The metal stent is a cobalt-chromium alloy, and the specific preparation method is as follows: Cleaning of stains: ultrasonically clean the metal bracket in acetone, anhydrous ethanol, and deionized water in order to remove impurities such as grease and fiber on the surface of the bracket. After cleaning, dry the bracket for later use. Acetone cleans organic pollutants, and anhydrous ethanol cleans inorganic pollutants. When both pollutants are involved, organic pollutants are generally cleaned first by default. Deionized water cleaning is placed last to clean the cleaning liquid of the first two steps. The container used is a polytetrafluoroethylene container or a beaker. The experimental containers required below are these two or other containers that will not react with the products contained.

[0048] Obtaining a scaffold sample with a hydroxyl-rich surface: Prepare a NaOH solution with a concentration of 3 mol / L, place the scaffold in a water bath of the NaOH solution at 60°C for 12 hours, rinse the scaffold with deionized water after the water bath and dry it to obtain a scaffold sample with a hydroxyl-rich surface.

[0049] Obtain a stent sample with a phytic acid layer coated on a hydroxyl-rich surface: prepare a phytic acid solution with a concentration of 5 mg / ml, use NaOH to adjust the pH value of the phytic acid solution to 5, place the stent sample with a hydroxyl-rich surface in a phytic acid solution at 50°C for 4 hours in a water bath, rinse the stent with deionized water after the water bath and dry it to obtain a stent sample with a phytic acid layer coated on the hydroxyl-rich surface.

[0050] Obtaining a stent sample with a polymer surface: Prepare a 2 mg / ml dopamine hydrochloride solution, in which the selected tris-base solution concentration is 15 mol / mL and the pH value is 8.5. Place the stent sample coated with a phytic acid layer in the solution and place it in a water bath at 37°C for 4 hours. After the water bath, rinse the stent with deionized water and dry it to obtain a stent sample coated with a polydopamine layer and a phytic acid layer on the hydroxyl-rich surface. Since the phytic acid layer and the dopamine layer are not completely coated with each other, the two are attached to each other in the gap between them, and work together to improve the adhesion strength.

[0051] Preparation of titanium dioxide solution: prepare an ammonium fluorotitanate solution with a concentration of 0.025 mol / L, prepare a boric acid solution with a concentration of 0.075 mol / L, and place the prepared ammonium fluorotitanate solution and boric acid solution in a water bath at 60°C for 6 hours. Mix the prepared ammonium fluorotitanate solution and boric acid solution in a volume ratio of 1:1, and use hydrofluoric acid to adjust the pH value of the mixed solution to 2.8.

[0052] Obtaining the final stent sample with a hydroxyl-rich surface, phytic acid, polymer and titanium dioxide coating: The stent sample coated with a phytic acid layer on the hydroxyl-rich surface was placed in a 50°C mixed solution for 30 minutes, and the stent was irradiated with ultraviolet light with a wavelength of 254 nm during the water bath. After the water bath, the stent was rinsed with deionized water and dried to obtain the final stent sample with a hydroxyl-rich surface, phytic acid and titanium dioxide coating.

[0053] Control group 1: The metal stent is directly coated with titanium dioxide.

[0054] The metal stent was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water in sequence. After cleaning, the stent was dried for later use.

[0055] An ammonium fluorotitanate solution with a concentration of 0.025 mol / L was prepared, and a boric acid solution with a concentration of 0.075 mol / L was prepared. The prepared ammonium fluorotitanate solution and the boric acid solution were placed in a water bath at 60° C. for 6 hours.

[0056] The ammonium fluorotitanate solution and the boric acid solution after the water bath are prepared are mixed in a volume ratio of 1:1, and the pH value of the mixed solution is adjusted to 2.8 with hydrofluoric acid. The stent sample is placed in a water bath in the mixed solution at 50°C for 0.5 hours, and the stent is irradiated with ultraviolet light with a wavelength of 254nm during the water bath. After the water bath, the stent is rinsed with deionized water and dried to obtain the final stent sample with titanium dioxide coating.

[0057] The stents having a hydroxyl-rich layer, an organic acid layer or a polymer layer, and a titanium dioxide layer prepared in Examples 1 to 4 were used as test samples, the stent having only a titanium dioxide layer prepared in Control Group 1 was used as Comparative Group 1, and the metal stent matrix identical to that in Examples 1 to 4 and Control Group 1 was used as a bare stent comparative group 2. The above stent samples were used to conduct an anticoagulation test.

[0058] After weighing the sample before the anticoagulation test on an electronic balance, put it into a container containing commercially available platelet-poor rabbit plasma (the anticoagulant is sodium citrate), add a certain amount of coagulant, shake it up and down repeatedly, observe visually, and after the rabbit whole blood coagulates, take out the sample, rinse it with deionized water, and dry it naturally. Weigh the weight of the bracket after the anticoagulation test on an electronic balance. The difference between the weight after the anticoagulation test and the weight before the anticoagulation test is divided by the weight before the anticoagulation test to obtain the mass increase rate (Table 1). According to the variable method, in order to exclude the interference of other factors, the concentration and temperature in each experiment should be kept the same or within a reasonable range as much as possible to avoid other factors interfering with the experimental results. The samples in this experiment were repeated many times to exclude data outside the reasonable range.

[0059] Table 1 Weight increase rate of samples before and after anticoagulation test

[0060] The data in the above table are average values ​​obtained from multiple samples. When calculating the average value, the data with large deviations are eliminated. As can be seen from Table 1, the mass increase rate of the bare stent is 8.1%, which is the largest in the test group. The mass increase rate of other samples with anticoagulant coating is significantly less than that of the bare stent, indicating that the stent with coating prepared in the embodiment of the present application has a significant anticoagulant effect. The weight increase rate of comparison group 1 is also relatively small. Although it is a significant improvement over comparison group 2, it is still insufficient compared to embodiments 1-4, indicating that the stent with polymer and organic acid layer has a more obvious anticoagulant effect.

[0061] The stent with a hydroxyl-rich layer, a phytic acid layer, and a titanium dioxide layer prepared in Example 1 was used as a test sample, and the stent with only a titanium dioxide layer prepared in Control Group 1 was used as a comparative group. The above stent samples were used to perform a test of completely inserting into a 0.027-inch inner diameter sheath tube and then completely withdrawing from the sheath tube for five times, and then the surface morphology of the stent was observed using a scanning electron microscope. The results are shown in FIG. Figure 1~Figure 4shown.

[0062] Depend on Figure 1 - 5 shows that the sample with the hydroxyl-rich layer, phytic acid layer, and titanium dioxide coating on the surface of the stent is still tightly connected to the metal stent after entering and exiting the sheath tube with an inner diameter of 0.027 inches five times. However, the sample directly coated with titanium dioxide coating has the phenomenon of separation from the metal stent after entering and exiting the sheath tube with an inner diameter of 0.027 inches five times. This shows that the stent prepared in Example 1 of the present application has a higher adhesion strength of the surface coating.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A coated blood flow guiding stent, comprising a metal stent and a titanium dioxide layer covering the surface of the metal stent; characterized in that: The metal support is covered with a hydroxyl-rich layer, the hydroxyl-rich layer is covered with an organic acid layer and / or a polymer layer, and the organic acid layer and / or the polymer layer is covered with a titanium dioxide layer.

2. A coated blood flow guiding stent according to claim 1, characterized in that: The metal stent composition includes one or more of cobalt-chromium alloy, platinum-tungsten alloy, nickel-titanium alloy, magnesium alloy, stainless steel, and titanium alloy.

3. The coated blood flow guiding stent according to claim 1, characterized in that: The components of the organic acid layer include one or more of phytic acid and tannic acid.

4. The coated blood flow guiding stent according to claim 1, characterized in that: The components of the polymer layer include one or more of polydopamine, chitosan, heparin, phosphorylcholine, and polyurethane.

5. A method for preparing a coated blood flow guiding stent, characterized in that: The method for preparing the coated blood flow guiding stent according to any one of claims 1 to 4 comprises the following steps: S1: Clean the metal bracket, dry it and set it aside; S2: preparing a NaOH solution, placing the metal stent in a water bath in the NaOH solution, rinsing the stent with deionized water after the water bath, and drying to obtain a metal stent sample with a hydroxyl-rich layer; S3: placing the metal stent sample with a hydroxyl-rich surface treated in step S2 into an organic acid or polymer solution for a water bath, and rinsing the stent with deionized water and drying it after the water bath to obtain a metal stent sample covered with an organic acid layer or a polymer layer; S4: preparing titanium dioxide solution; S5: placing the metal stent treated in step S3 into the titanium dioxide solution in step S4 for a water bath. After the water bath, rinse the stent with deionized water and dry it to obtain a metal stent sample covered with a titanium dioxide layer.

6. The method for preparing a coated blood flow guiding stent according to claim 5, characterized in that: The cleaning process in S1 is ultrasonic cleaning in acetone, anhydrous ethanol, and deionized water in sequence; the concentration of the NaOH solution in S2 is 0.01-10 mol / L, the water bath temperature is 20-80°C, and the water bath time is 0-72h.

7. The method for preparing a coated blood flow guiding stent according to claim 5, characterized in that: When preparing the metal stent sample with organic acid layer in S3, prepare a phytic acid solution with a concentration of 0.01 mg / ml~10 mg / ml, adjust the pH value of the phytic acid solution to 2-7 using NaOH, and place the stent sample with hydroxyl-rich surface in a water bath in the phytic acid solution at 20-80°C for 0-72 hours.

8. The method for preparing a coated blood flow guiding stent according to claim 5, characterized in that: When preparing the metal stent sample with organic acid layer in S3, prepare 1-10 mg / ml tannic acid solution, wherein the concentration of Tris-HCl solution is 1-5 mg / ml, and the pH value is adjusted to 8-11 by NaOH, and the stent sample with hydroxyl-rich surface is placed in the solution and placed in a water bath at 0-70°C for 1-8 hours.

9. The method for preparing a coated blood flow guiding stent according to claim 5, characterized in that: When preparing the metal stent sample of the polymer layer in S3, a 2 mg / ml dopamine hydrochloride solution is prepared, wherein the tris-base solution concentration is selected to be 15 mol / mL and the pH value is 8.

5. The stent sample with a hydroxyl-rich surface is placed in the solution and placed in a water bath at 37°C for 6 hours.

10. The method for preparing a coated blood flow guiding stent according to claim 5, characterized in that: The preparation process in S4 is as follows: prepare an ammonium fluorotitanate solution with a concentration of 0.005-0.35 mol / L, prepare a boric acid solution with a concentration of 0.005-0.5 mol / L, place the prepared ammonium fluorotitanate solution and the boric acid solution in a water bath at 60°C for 12 hours, mix the prepared ammonium fluorotitanate solution and the boric acid solution in a volume ratio of 1:1, and use hydrofluoric acid to adjust the pH value of the mixed solution to 2.8 to obtain a titanium dioxide solution; the water bath temperature in S5 is 20-80°C, the water bath time is 0-24 hours, and the bracket sample is irradiated with ultraviolet light with a wavelength of 254nm during the water bath.

Citation Information

Cited By

  • Antibacterial and anticoagulant coating composition, antibacterial and anticoagulant coating, preparation method of antibacterial and anticoagulant coating and medical material

    CN119868669A

  • An antibacterial, anticoagulant coating composition, an antibacterial, anticoagulant coating and a method for producing the same, a medical material

    CN119868669B