A preparation method and application of a catalyst for EEP synthesis

By combining the frame material of the three-dimensional web frame structure with the porous support alumina, KNO3 is bound, the problem of K2O separation is solved, the catalyst life is extended, the EEP production cost is reduced, and the catalytic activity is maintained.

CN118874542BActive Publication Date: 2024-12-03SHENZHEN PRECHEM FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411384359.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

In the supported alkali metal catalysts used in EEP synthesis in the prior art, K2O is prone to detachment, resulting in a decrease in the number of catalyst reuses and an increase in production costs.

Method used

KNO3 is bound through the frame material of the three-dimensional web frame structure and forms a stable cooperation with the porous support alumina, improving the fixation of K2O and extending the service life of the catalyst.

Benefits of technology

The number of reuses of catalysts is increased, the cost of EEP is reduced, and the channel is generated through the roasting process to avoid the blockage of potassium oxide and maintain catalytic activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the field of chemical synthesis, and in particular to a method for preparing a catalyst for EEP synthesis and its application, the method for preparing a catalyst comprises the following steps: S1, 1,3,5-tris (4-aminophenyl) benzene and 2,5-dimethoxy terephthalaldehyde are added to an organic solvent, and a heating reaction is generated to form a framework material; S2, the framework material is placed in a container and ethanol is added, and then a nitrate is added to heat the reaction to generate a load liquid; S3, an aluminum inorganic salt and urea are generated into an aluminum precursor, and the aluminum precursor is added to the load liquid and stirred evenly, and a porous carrier is formed by roasting; S4, a porous carrier is added to ethanol, ethyl acrylate and EEP mixed solution, and a catalyst is obtained by roasting after impregnation and drying. The present invention restrains KNO3 by a framework material of a three-dimensional mesh frame structure, and then a stable coordination is formed by using the framework material and a porous carrier alumina, so as to improve the fixation of K2O, and effectively avoid the falling off of K2O.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical synthesis, and in particular relates to a preparation method of a catalyst for EEP synthesis and application thereof. Background Art

[0002] Ethyl 3-ethoxypropionate (EEP) is an important organic solvent and organic synthesis intermediate. It has good solubility for a wide range of coating polymers. It can replace traditional alcohol ether and ether ester solvents and has better performance. It has a great potential application market in the coating industry and microelectronics industry (photoresist stripping agent, diluent).

[0003] At present, in the process of preparing EEP, supported alkali metal catalysts are mostly used, generally KNO3 is used for preparation. During the preparation, KNO3 is loaded on a porous carrier and calcined to generate strong alkaline sites. However, the strong alkaline sites of K2O generated in the catalyst are easily separated from the carrier, which reduces the number of times the catalyst is reused. Therefore, in the process of producing EEP, new catalysts need to be frequently replaced, resulting in an increase in the production cost of EEP. Summary of the invention

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a catalyst for EEP synthesis and its application, wherein KNO3 is bound by a framework material of a three-dimensional mesh frame structure, and then the framework material is used to form a stable combination with a porous carrier alumina, thereby improving the fixation of K2O and effectively preventing K2O from falling off.

[0005] The specific technical solution adopted by the present invention is:

[0006] A method for preparing a catalyst for EEP synthesis comprises the following steps:

[0007] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into an organic solvent, heat to 90-120° C. and react for 2-4 hours to generate a framework material;

[0008] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 50-80°C and react for 1-2 h to generate a loading liquid;

[0009] S3, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding the aluminum precursor to a loading liquid, stirring evenly, and calcining to form a porous carrier;

[0010] S4. Add the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immerse for 4-8 hours, dry and calcine to obtain a catalyst.

[0011] The mass ratio of the 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 15-20:10-20.

[0012] The mass ratio of the nitrate to the aluminum precursor is 10-20:100.

[0013] The molar ratio of the framework material to the nitrate is 1-2:1.

[0014] The organic solvent includes any one of ethanol, methanol, toluene, cyclohexane and methylcyclohexane.

[0015] The step S3 further comprises the following steps:

[0016] S311, adding 1H,1H,2H,2H-perfluorodecyl mercaptan to an organic solvent and stirring evenly to obtain a modification solution;

[0017] S312. Aluminum inorganic salt and urea are reacted under hydrothermal conditions to generate an aluminum precursor, the modification liquid is added to the aluminum precursor and stirred evenly, and then added to the load liquid and stirred evenly, reacted at room temperature for 4-6 hours, and then calcined to form a porous carrier.

[0018] The volume ratio of the 1H,1H,2H,2H-perfluorodecyl mercaptan to the organic solvent is 2-4:1000.

[0019] An application of a catalyst for EEP synthesis comprises the following steps:

[0020] A. preparing catalyst;

[0021] B. synthesizing EEP using the catalyst;

[0022] Step A includes the following steps:

[0023] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into an organic solvent, heat to 90-120° C. and react for 2-4 hours to generate a framework material;

[0024] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 40-80°C and react for 1-2 h to generate a loading liquid;

[0025] S3, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding the aluminum precursor to a loading liquid, stirring evenly, and calcining to form a porous carrier;

[0026] S4, adding the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immersing for 4-8 hours, drying and calcining to obtain a catalyst;

[0027] Step B includes the following steps:

[0028] S5. Add ethanol and ethyl acrylate into a reaction kettle, then add hydroquinone monomethyl ether and a catalyst, mix well, and react at 50-60° C. for 2-4 hours to obtain an EEP finished product.

[0029] The raw materials of the EEP include, by mass fraction, 120-150 parts of ethanol, 90-100 parts of ethyl acrylate, 2-4 parts of catalyst, and 0.1-0.2 parts of hydroquinone monomethyl ether.

[0030] The beneficial effects of the present invention are:

[0031] 1. In the present invention, KNO3 is bound by a framework material of a three-dimensional mesh frame structure, and then the framework material is used to form a stable combination with a porous carrier alumina, thereby improving the fixation of K2O and effectively preventing the shedding of K2O, so that the catalyst in the present invention still has a high catalytic activity after multiple uses, increasing the number of times the catalyst is reused and reducing the production cost of EEP.

[0032] 2. In the prior art, a porous carrier is generally prepared first, and then the catalyst and the carrier are attached. In the present invention, the catalyst precursor and the carrier precursor are first mixed, and then calcined to form a porous carrier loaded with the catalyst. Through this method, on the one hand, the bonding stability between the catalyst and the carrier can be further increased. On the other hand, through this method, during the calcination process, channels for reactants to pass through are generated inside the carrier, thereby preventing potassium oxide from blocking the pores of the carrier and causing the activity of the catalyst to decrease.

[0033] 3. By adding the hydrophobic group 1H,1H,2H,2H-perfluorodecyl mercaptan, the agglomeration phenomenon in the process of preparing porous supports from aluminum precursors can be effectively improved, thereby improving the quality of the porous supports. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. 1. Specific embodiments

[0036] Example 1

[0037] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 100°C for 3h to react and generate a framework material;

[0038] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 1:1;

[0039] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 60°C and react for 1.5 h to generate a loading liquid;

[0040] The molar ratio of the framework material to the nitrate is 1.5:1;

[0041] S311, adding 3 parts by volume of 1H,1H,2H,2H-perfluorodecyl mercaptan to 1000 parts by volume of ethanol and stirring evenly to obtain a modification solution;

[0042] S312, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding a modification solution to the aluminum precursor and stirring evenly, adding 1 ml of the modification solution to each mg of the precursor, and then adding the modified solution to the loading solution and stirring evenly, reacting at room temperature for 5 hours, and then calcining at 750°C to form a porous carrier;

[0043] The mass ratio of nitrate to aluminum precursor is 15:100;

[0044] S4. Add the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immerse for 6 hours, dry and calcine for 5 hours to obtain a catalyst.

[0045] Example 2

[0046] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 90°C and react for 4 hours to generate a framework material;

[0047] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 15:20;

[0048] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 50°C for 2 h to generate a loading solution;

[0049] The molar ratio of the framework material to the nitrate is 1:1;

[0050] S311, adding 2 parts by volume of 1H,1H,2H,2H-perfluorodecyl mercaptan to 1000 parts by volume of ethanol and stirring evenly to obtain a modification solution;

[0051] S312, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding a modification liquid to the aluminum precursor and stirring evenly, adding 1 ml of the modification liquid to each mg of the precursor, and then adding the modified liquid to the loading liquid and stirring evenly, reacting at room temperature for 5 hours, and then calcining at 650°C to form a porous carrier;

[0052] The mass ratio of nitrate to aluminum precursor is 10:100;

[0053] S4. Add the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immerse for 4 hours, dry and calcine for 6 hours to obtain a catalyst.

[0054] Example 3

[0055] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 120°C and react for 2h to generate a framework material;

[0056] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 15:20;

[0057] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 80°C for 1 h to generate a loading liquid;

[0058] The molar ratio of the framework material to the nitrate is 1:2;

[0059] S311, adding 4 parts by volume of 1H,1H,2H,2H-perfluorodecyl mercaptan to 1000 parts by volume of ethanol and stirring evenly to obtain a modification solution;

[0060] S312, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding a modification liquid to the aluminum precursor and stirring evenly, adding 1 ml of the modification liquid to each mg of the precursor, and then adding the modified liquid to the loading liquid and stirring evenly, reacting at room temperature for 5 hours, and then calcining at 800°C to form a porous carrier;

[0061] The mass ratio of nitrate to aluminum precursor is 20:100;

[0062] S4. Add the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immerse for 8 hours, dry and calcine for 4 hours to obtain a catalyst.

[0063] Example 4

[0064] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 110°C and react for 3.5 hours to generate a framework material;

[0065] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 15:18;

[0066] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 675℃ and react for 1.2 h to generate a loading liquid;

[0067] The molar ratio of the framework material to the nitrate is 1.4:1;

[0068] S311, adding 2.5 parts by volume of 1H,1H,2H,2H-perfluorodecyl mercaptan to 1000 parts by volume of ethanol and stirring evenly to obtain a modification solution;

[0069] S312, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding a modification solution to the aluminum precursor and stirring evenly, adding 1 ml of the modification solution to each mg of the precursor, and then adding the modified solution to the loading solution and stirring evenly, reacting at room temperature for 4 hours, and then calcining at 620°C to form a porous carrier;

[0070] The mass ratio of nitrate to aluminum precursor is 18:100;

[0071] S4. Add the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immerse for 6 hours, dry and calcine for 5 hours to obtain a catalyst.

[0072] Example 5

[0073] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 95°C for 3h to react and generate a framework material;

[0074] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 1.6:1;

[0075] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 70°C and react for 1.2h to generate a loading liquid;

[0076] The molar ratio of the framework material to the nitrate is 1.6:1;

[0077] S311, adding 2 parts by volume of 1H,1H,2H,2H-perfluorodecyl mercaptan to 1000 parts by volume of ethanol and stirring evenly to obtain a modification solution;

[0078] S312, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding a modification solution to the aluminum precursor and stirring evenly, adding 1 ml of the modification solution to each mg of the precursor, and then adding the modified solution to the loading solution and stirring evenly, reacting at room temperature for 5 hours, and then calcining at 720°C to form a porous carrier;

[0079] The mass ratio of nitrate to aluminum precursor is 12:100;

[0080] S4, adding the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immersing for 6 hours, drying and calcining for 5 hours to obtain a catalyst;

[0081] Comparative Example 1

[0082] S1, adding nitrate to water and mixing evenly to form a loading solution;

[0083] S2, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding the aluminum precursor to a loading liquid, stirring evenly, and calcining at 750° C. to form a porous carrier;

[0084] The mass ratio of nitrate to aluminum precursor is 15:100;

[0085] S3, adding the porous carrier into a mixed solution of ethanol, ethyl acrylate and EEP, immersing for 6 hours, drying and calcining for 5 hours to obtain a catalyst;

[0086] Comparative Example 2

[0087] S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into ethanol, heat to 100°C for 3h to react and generate a framework material;

[0088] The mass ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 1:1;

[0089] S2, put the framework material into a container and add ethanol, then add nitrate and stir to form a suspension, then heat to 60°C and react for 1.5 h to generate a loading liquid;

[0090] The molar ratio of the framework material to the nitrate is 1.5:1;

[0091] S3, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, and calcining the precursor at 750° C. to form a porous carrier;

[0092] S4, immersing the porous support in the loading liquid for 4 hours, then taking out the surface of the porous support and adding it into a mixed solution of ethanol, ethyl acrylate and EEP, immersing for 6 hours, drying and calcining for 5 hours to obtain a catalyst;

[0093] The mass ratio of nitrate to aluminum precursor is 15:100;

[0094] 2. Performance Test

[0095] The catalysts prepared in Examples 1-5 and Comparative Examples 1-2 were used to prepare EEP. After the preparation, the catalysts were taken out, and then the EEP was prepared again. This process was repeated several times, and the conversion rate of ethyl acrylate in each reaction was tested. The test results are shown in Table 1.

[0096] The preparation process of EEP is as follows: 123 parts of ethanol and 92 parts of ethyl acrylate are added into a reactor, and then 0.1 parts of hydroquinone monomethyl ether and 3 parts of a catalyst are added, mixed evenly, and reacted at 55° C. for 2 hours to obtain the finished EEP product.

[0097] Table 1

[0098]

[0099] It can be seen from Table 1 that the conversion rate of ethyl acrylate of the catalysts prepared in Examples 1-5 is still above 96% when used for the fifth time, while the catalysts prepared in Comparative Examples 1 and 2 have a higher conversion rate of ethyl acrylate at the beginning during use, but after multiple uses, the conversion rate of ethyl acrylate is only about 80-90%, and cannot be used further.

[0100] The conversion rate of ethyl acrylate of the catalyst in Comparative Example 1 decreased rapidly, and although the frame material was used in Comparative Example 2 to slow down the rate of decrease of the conversion rate of ethyl acrylate, it was still less than 90% after 5 uses.

[0101] From the above, it can be seen that the catalyst in the present invention has a good bonding degree with the carrier. This is because KNO3 is bound by the framework material of the three-dimensional mesh frame structure, and the framework material is used to form a stable combination with the porous carrier alumina, thereby improving the fixation of K2O and effectively preventing K2O from falling off.

[0102] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate, It is characterized in that The following steps are involved: S1. Add 1,3,5-tris(4-aminophenyl)benzene and 2,5-dimethoxyterephthalaldehyde into an organic solvent, heat to 90-120° C. and react for 2-4 hours to generate a framework material; S2, placing the framework material in a container and adding an organic solvent, then adding potassium nitrate and stirring to form a suspension, and then heating to 50-80°C for 1-2 h to generate a loading liquid; S3, generating an aluminum precursor by reacting an aluminum inorganic salt with urea under hydrothermal conditions, adding the aluminum precursor to a loading liquid, stirring evenly, and calcining to form a porous carrier; S4, adding the porous carrier into a mixed solution of ethanol, ethyl acrylate and ethyl 3-ethoxypropionate, immersing for 4-8 hours, drying and calcining to obtain a catalyst; The step S3 specifically comprises the following steps: S311, adding 1H,1H,2H,2H-perfluorodecyl mercaptan to an organic solvent and stirring evenly to obtain a modification solution; S312. Aluminum inorganic salt and urea are reacted under hydrothermal conditions to generate an aluminum precursor, the modification liquid is added to the aluminum precursor and stirred evenly, and then added to the load liquid and stirred evenly, reacted at room temperature for 4-6 hours, and then calcined to form a porous carrier.

2. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate according to claim 1, It is characterized in that The mass ratio of the 1,3,5-tris(4-aminophenyl)benzene to 2,5-dimethoxyterephthalaldehyde is 15-20:10-20.

3. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate according to claim 1, It is characterized in that The mass ratio of the potassium nitrate to the aluminum precursor is 10-20:

100.

4. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate according to claim 1, It is characterized in that The molar ratio of the framework material to potassium nitrate is 1-2:

1.

5. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate according to claim 1, It is characterized in that The organic solvents described in step S1, step S2 and step S311 are all ethanol.

6. A method for preparing a catalyst for the synthesis of ethyl 3-ethoxypropionate according to claim 1, It is characterized in that The volume ratio of the 1H,1H,2H,2H-perfluorodecyl mercaptan to the organic solvent is 2-4:1000.

7. Use of the catalyst obtained by the preparation method according to any one of claims 1 to 6 in the synthesis of ethyl 3-ethoxypropionate, It is characterized in that The following steps are involved: Add ethanol and ethyl acrylate into a reaction kettle, then add hydroquinone monomethyl ether and the above catalyst, mix well, and react at 50-60° C. for 2-4 hours to obtain ethyl 3-ethoxypropionate as a finished product.

8. The use according to claim 7, It is characterized in that The raw materials for synthesizing ethyl 3-ethoxypropionate include, by mass fraction, 120-150 parts of ethanol, 90-100 parts of ethyl acrylate, 2-4 parts of catalyst and 0.1-0.2 parts of hydroquinone monomethyl ether.