Steel belt for electric chain saw and production method thereof

By using steel with moderate carbon content and cemented carbide teeth with high tungsten content, combined with vibration-absorbing layer and lubricating chute design, the problems of wear and vibration noise of steel strips for electric chain saws are solved, and more efficient and durable steel is achieved. With performance.

CN118875387AInactive Publication Date: 2024-11-01ANHUI CHUJIANG SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933352.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The steel belt used for electric chain saws will wear after long-term high-strength use, and it needs to be inspected and replaced regularly. The friction between the steel belt and the chain will produce greater vibration and noise, affecting working efficiency and comfort.

Method used

Matrix steel strips are made of steel with a carbon content of 0.6%-0.8%. The cemented carbide teeth are made of 85%-95% tungsten-cobalt carbide, and are between the matrix steel strip and the cemented carbide teeth. Add a vibration-absorbing layer, and a lubricating chute is provided along the length of the steel strip to store lubricant, reduce friction and vibration, and improve wear resistance and service life.

Benefits of technology

It effectively reduces friction and vibration between the steel belt and the chain, extends the service life of the steel belt, reduces noise, and improves working efficiency and comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875387A_ABST
    Figure CN118875387A_ABST
Patent Text Reader

Abstract

The invention provides a steel belt for an electric chain saw and a production method thereof, and relates to the field of steel belts for electric chain saws. The steel belt for the electric chain saw comprises a base body steel belt, hard alloy teeth, a vibration reduction layer and a lubricating groove, the base body steel belt is made of steel with the carbon content being 0.6%-0.8% and formed through a cold rolling or hot rolling process, the hard alloy teeth are fixed to the surface of the base body steel belt, and the hard alloy teeth are made of tungsten-cobalt hard alloy with the tungsten content being 85%-95%. High-strength steel with moderate carbon content is selected and combined with a cold rolling or hot rolling process to form a matrix steel belt, the strength and toughness of the steel belt are guaranteed, the hard alloy teeth are made of tungsten-cobalt hard alloy with high tungsten content, the hard alloy teeth are manufactured through a sintering process and subjected to chemical passivation treatment, the wear resistance of the teeth is improved, and the service life of the teeth is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel belts for electric chain saws, in particular to a steel belt for an electric chain saw and a production method thereof. Background Art

[0002] The steel belt for electric chain saw is a key component specially designed for electric chain saw. It is usually made of high-strength steel with high wear resistance and high toughness. Its basic structure includes:

[0003] Base steel belt: The base steel belt is the core part of the entire steel belt. It is made of high-quality steel and formed by cold rolling or hot rolling process. The base steel belt needs to have sufficient strength and flexibility to withstand the tension of the chain saw when it is running at high speed and the impact force when cutting. Carbide teeth: Carbide teeth are fixed on the surface of the base steel belt by welding or brazing. Carbide teeth are the cutting part of the steel belt. They are usually made of tungsten-cobalt carbide. They have extremely high hardness and wear resistance and can effectively cut wood. Chain connection holes and chains: There are several chain connection holes distributed on the steel belt for fixing the chain. The chain is a key component of the steel belt transmission for electric chain saws. It is firmly connected to the steel belt through these connection holes, so that the steel belt can rotate quickly with the movement of the electric chain saw. Lubrication system: In order to reduce friction and extend the service life of the steel belt, electric chain saws are usually equipped with a lubrication system to lubricate the steel belt and chain regularly.

[0004] Although electric chain saw steel belts have many advantages in design and use, they also have some disadvantages:

[0005] Even though carbide teeth are highly wear-resistant, they will still wear out after long-term, intensive use and need to be checked and replaced regularly. This not only increases maintenance costs, but may also cause downtime during use, affecting work efficiency. When electric chain saws are running at high speeds, the friction between the steel belt and the chain will produce large vibrations and noise. This not only affects the comfort of the operator, but may also have an adverse effect on the surrounding environment. Although the lubrication system can alleviate this situation to a certain extent, it cannot completely eliminate it. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In view of the deficiencies in the prior art, the present invention provides a steel belt for an electric chain saw and a production method thereof, which solves the problem that after long-term high-intensity use, the steel belt will still wear out and need to be regularly inspected and replaced; and the friction between the steel belt and the chain will generate large vibrations and noise.

[0008] (II) Technical solution

[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions: A steel belt for an electric chain saw, comprising:

[0010] Base steel belt, carbide teeth, vibration damping layer and lubrication groove;

[0011] The base steel strip is made of steel with a carbon content of 0.6%-0.8% and is formed by a cold rolling or hot rolling process. The carbide teeth are fixed on the surface of the base steel strip. The carbide teeth are made of tungsten-cobalt carbide with a tungsten content of 85%-95%. The vibration damping layer is located between the base steel strip and the carbide teeth to reduce the friction and vibration between the steel strip and the chain. The lubrication groove is arranged along the length direction of the base steel strip for storing lubricant to ensure continuous lubrication of the steel strip during operation. The width of the lubrication groove is 2mm-4mm and the depth is 1mm-2mm.

[0012] Preferably, the vibration damping layer is made of rubber, silicone or polyurethane material with a thickness of 0.5 mm-1 mm, and nano-scale carbon fibers are added to the vibration damping layer, and the content of the nano-scale carbon fibers is less than 1%, so as to further enhance the vibration damping effect.

[0013] Preferably, the cross-section of the lubrication groove is V-shaped to improve the storage and distribution efficiency of the lubricant, and the surface of the cemented carbide tooth is chemically passivated to increase its wear resistance and service life.

[0014] A method for producing a steel strip for an electric chain saw comprises the following steps:

[0015] S1. Select high-strength and high-toughness steel with a carbon content of 0.6%-0.8%;

[0016] S2. The steel is heated to 500°C-700°C for annealing to improve its plasticity and toughness, and the steel is processed into a steel strip with a thickness of 2mm-4mm by cold rolling or hot rolling, and the steel strip is cut into the required length and subjected to shaping treatment;

[0017] S3. Select tungsten-cobalt cemented carbide materials with a tungsten content of 85%-95%, sinter the cemented carbide materials at a temperature range of 1400℃-1600℃ to form cemented carbide teeth, and perform precision machining and trimming on the cemented carbide teeth to ensure the accuracy of their size and shape;

[0018] S4. Select rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm, and fix the vibration-damping material on the surface of the base steel belt by hot pressing or gluing at 200℃-250℃ for 2-3 minutes;

[0019] S5. Lubrication grooves are set along the length direction on the base steel belt. The width of the lubrication grooves is 2mm-4mm and the depth is 1mm-2mm. They are formed by machining or etching process. Mineral oil or synthetic oil is used as lubricant. Lubricant is added to the lubrication grooves to ensure continuous lubrication of the steel belt during operation.

[0020] Preferably, the surface of the cemented carbide tooth is subjected to chemical passivation treatment, the passivating agent is a fluorine-containing compound solution, the treatment temperature is 25° C.-30° C., and the treatment time is 15-20 minutes, so as to increase its wear resistance and service life.

[0021] Preferably, the carbide teeth are fixed to the base steel strip by a high temperature welding process, the welding temperature is 800°C-1000°C, the welding time is 5-10 minutes, and the rolling speed of the cold rolling process is 2m / min-5m / min to ensure the flatness and uniformity of the steel strip.

[0022] Preferably, the etching process is performed using an acidic solution for 10-15 minutes to form a lubrication groove with excellent wear resistance, and the sintering process has a pressure of 100MPa-200MPa to ensure the density and strength of the cemented carbide teeth.

[0023] Preferably, the pressure of the hot pressing process is 5 MPa-10 MPa to ensure good bonding between the vibration damping layer and the base steel strip.

[0024] (III) Beneficial effects

[0025] The present invention provides a steel belt for an electric chain saw and a production method thereof. The steel belt has the following beneficial effects:

[0026] The base steel belt is formed by selecting high-strength steel with an appropriate carbon content and combining it with a cold rolling or hot rolling process to ensure the strength and toughness of the steel belt. The cemented carbide teeth are made of tungsten-cobalt cemented carbide with a high tungsten content. They are made through a sintering process and chemically passivated to enhance the wear resistance and service life of the teeth. The vibration-damping layer uses a high-elastic material with an appropriate thickness and is firmly combined with the base steel belt through a hot pressing or bonding process to effectively reduce the friction and vibration between the steel belt and the chain. The lubrication groove is reasonably designed and formed through a mechanical processing or etching process, and lubricant is added to the groove to ensure continuous lubrication of the steel belt during operation and increase the service life of the steel belt. The entire production process includes strict temperature, pressure and time control to ensure the quality and performance of each step, thereby providing an efficient, durable steel belt for electric chain saws with low vibration and noise and a production method thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Embodiment 1:

[0030] like Figure 1 As shown, an embodiment of the present invention provides a steel belt for an electric chain saw, comprising a base steel belt, carbide teeth, a vibration-damping layer and a lubrication groove;

[0031] The base steel belt is made of steel with a carbon content of 0.6% and is formed by a cold rolling or hot rolling process. The carbide teeth are fixed on the surface of the base steel belt. The carbide teeth are made of tungsten-cobalt carbide with a tungsten content of 85%. The vibration reduction layer is located between the base steel belt and the carbide teeth to reduce the friction and vibration between the steel belt and the chain. The lubrication groove is arranged along the length direction of the base steel belt to store lubricants to ensure that the steel belt is continuously lubricated during operation. The width of the lubrication groove is 2mm-4mm and the depth is 1mm-2mm. The vibration reduction layer is made of rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm. Nano-scale carbon fibers are added to the vibration reduction layer, and the content of nano-scale carbon fibers is less than 1% to further enhance its vibration reduction effect. The cross-section of the lubrication groove is V-shaped to improve the storage and distribution efficiency of the lubricant. The surface of the carbide teeth is chemically passivated to increase its wear resistance and service life.

[0032] A method for producing a steel strip for an electric chain saw comprises the following steps:

[0033] S1. Select high-strength and high-toughness steel with a carbon content of 0.6%.

[0034] S2. The steel is heated to 500°C-700°C for annealing to improve its plasticity and toughness. The steel is processed into a steel strip with a thickness of 2mm-4mm through a cold rolling or hot rolling process. The steel strip is cut into the required length and subjected to shaping treatment.

[0035] S3. Select tungsten-cobalt cemented carbide material with a tungsten content of 85%, sinter the cemented carbide material within the temperature range of 1400℃-1600℃ to form cemented carbide teeth, and perform precision machining and trimming on the cemented carbide teeth to ensure the accuracy of their size and shape. The surface of the cemented carbide teeth is chemically passivated, the passivating agent is a fluorine-containing compound solution, the treatment temperature is 25℃-30℃, and the treatment time is 15-20 minutes to increase its wear resistance and service life. The cemented carbide teeth are fixed on the base steel strip through a high-temperature welding process, the welding temperature is 800℃-1000℃, the welding time is 5-10 minutes, and the rolling speed of the cold rolling process is 2m / min-5m / min to ensure the flatness and uniformity of the steel strip.

[0036] S4. Select rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm, and fix the vibration-damping material on the surface of the base steel strip through a hot pressing or gluing process at 200℃-250℃. The hot pressing time is 2-3 minutes, and the pressure of the hot pressing process is 5MPa-10MPa to ensure good bonding between the vibration-damping layer and the base steel strip.

[0037] S5. Lubrication grooves are set along the length direction of the base steel strip. The width of the lubrication grooves is 2mm-4mm and the depth is 1mm-2mm. They are formed by mechanical processing or etching process. Mineral oil or synthetic oil is selected as lubricant. Lubricant is added to the lubrication grooves to ensure continuous lubrication of the steel strip during operation. The etching process is carried out with an acidic solution. The etching time is 10-15 minutes to form a lubrication groove with excellent wear resistance. The pressure of the sintering process is 100MPa-200MPa to ensure the density and strength of the cemented carbide teeth.

[0038] Embodiment 2:

[0039] like Figure 1 As shown, an embodiment of the present invention provides a steel belt for an electric chain saw, comprising a base steel belt, carbide teeth, a vibration-damping layer and a lubrication groove;

[0040] The base steel belt is made of steel with a carbon content of 0.8% and is formed by a cold rolling or hot rolling process. The carbide teeth are fixed on the surface of the base steel belt. The carbide teeth are made of tungsten-cobalt carbide with a tungsten content of 95%. The vibration reduction layer is located between the base steel belt and the carbide teeth to reduce the friction and vibration between the steel belt and the chain. The lubrication groove is arranged along the length direction of the base steel belt to store lubricants to ensure that the steel belt is continuously lubricated during operation. The width of the lubrication groove is 2mm-4mm and the depth is 1mm-2mm. The vibration reduction layer is made of rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm. Nano-scale carbon fibers are added to the vibration reduction layer, and the content of nano-scale carbon fibers is less than 1% to further enhance its vibration reduction effect. The cross-section of the lubrication groove is V-shaped to improve the storage and distribution efficiency of the lubricant. The surface of the carbide teeth is chemically passivated to increase its wear resistance and service life.

[0041] A method for producing a steel strip for an electric chain saw comprises the following steps:

[0042] S1. Select high-strength and high-toughness steel with a carbon content of 0.8%.

[0043] S2. The steel is heated to 500°C-700°C for annealing to improve its plasticity and toughness. The steel is processed into a steel strip with a thickness of 2mm-4mm through a cold rolling or hot rolling process. The steel strip is cut into the required length and subjected to shaping treatment.

[0044] S3. Use tungsten-cobalt cemented carbide material with a tungsten content of 95%, sinter the cemented carbide material within the temperature range of 1400℃-1600℃ to form cemented carbide teeth, and perform precision machining and trimming on the cemented carbide teeth to ensure the accuracy of their size and shape. The surface of the cemented carbide teeth is chemically passivated, the passivating agent is a fluorine-containing compound solution, the treatment temperature is 25℃-30℃, and the treatment time is 15-20 minutes to increase its wear resistance and service life. The cemented carbide teeth are fixed on the base steel strip through a high-temperature welding process, the welding temperature is 800℃-1000℃, the welding time is 5-10 minutes, and the rolling speed of the cold rolling process is 2m / min-5m / min to ensure the flatness and uniformity of the steel strip.

[0045] S4. Select rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm, and fix the vibration-damping material on the surface of the base steel strip through a hot pressing or gluing process at 200℃-250℃. The hot pressing time is 2-3 minutes, and the pressure of the hot pressing process is 5MPa-10MPa to ensure good bonding between the vibration-damping layer and the base steel strip.

[0046] S5. Lubrication grooves are set along the length direction of the base steel strip. The width of the lubrication grooves is 2mm-4mm and the depth is 1mm-2mm. They are formed by mechanical processing or etching process. Mineral oil or synthetic oil is selected as lubricant. Lubricant is added to the lubrication grooves to ensure continuous lubrication of the steel strip during operation. The etching process is carried out with an acidic solution. The etching time is 10-15 minutes to form a lubrication groove with excellent wear resistance. The pressure of the sintering process is 100MPa-200MPa to ensure the density and strength of the cemented carbide teeth.

[0047] Table 1: Performance parameter comparison table

[0048] Performance / Parameters Embodiment 1 Embodiment 2 Carbon content of base steel strip 0.6% 0.8% Tungsten content in cemented carbide teeth 85% 95% Thickness of vibration damping layer 0.5mm-1mm 0.5mm-1mm Vibration damping layer material Rubber, silicone or polyurethane Rubber, silicone or polyurethane Nano carbon fiber content in the vibration damping layer <1% <1%

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A steel belt for an electric chain saw, characterized in that: include: Base steel belt, carbide teeth, vibration damping layer and lubrication groove; The base steel strip is made of steel with a carbon content of 0.6%-0.8% and is formed by a cold rolling or hot rolling process. The carbide teeth are fixed on the surface of the base steel strip. The carbide teeth are made of tungsten-cobalt carbide with a tungsten content of 85%-95%. The vibration damping layer is located between the base steel strip and the carbide teeth to reduce friction and vibration between the steel strip and the chain. The lubrication groove is arranged along the length direction of the base steel strip for storing lubricant. The width of the lubrication groove is 2mm-4mm and the depth is 1mm-2mm.

2. The steel belt for an electric chain saw according to claim 1, characterized in that: The vibration-damping layer is made of rubber, silicone or polyurethane material with a thickness of 0.5 mm to 1 mm. Nano-scale carbon fibers are added to the vibration-damping layer, and the content of the nano-scale carbon fibers is less than 1%.

3. The steel belt for an electric chain saw according to claim 1, characterized in that: The cross section of the lubrication groove is V-shaped to improve the storage and distribution efficiency of the lubricant, and the surface of the cemented carbide tooth is chemically passivated to increase its wear resistance and service life.

4. A method for producing a steel strip for an electric chain saw, characterized in that: The following steps are involved: S1. Select high-strength and high-toughness steel with a carbon content of 0.6%-0.8%; S2. The steel is heated to 500°C-700°C for annealing to improve its plasticity and toughness, and the steel is processed into a steel strip with a thickness of 2mm-4mm by cold rolling or hot rolling, and the steel strip is cut into the required length and subjected to shaping treatment; S3. Select tungsten-cobalt cemented carbide materials with a tungsten content of 85%-95%, sinter the cemented carbide materials at a temperature range of 1400℃-1600℃ to form cemented carbide teeth, and perform precision machining and trimming on the cemented carbide teeth to ensure the accuracy of their size and shape; S4. Select rubber, silicone or polyurethane material with a thickness of 0.5mm-1mm, and fix the vibration-damping material on the surface of the base steel belt by hot pressing or gluing at 200℃-250℃ for 2-3 minutes; S5. Lubrication grooves are set along the length direction on the base steel belt. The width of the lubrication grooves is 2mm-4mm and the depth is 1mm-2mm. They are formed by machining or etching process. Mineral oil or synthetic oil is used as lubricant. Lubricant is added to the lubrication grooves to ensure continuous lubrication of the steel belt during operation.

5. The method for producing a steel strip for an electric chain saw according to claim 4, characterized in that: The surface of the cemented carbide tooth is chemically passivated, the passivating agent is a fluorine-containing compound solution, the treatment temperature is 25° C.-30° C., and the treatment time is 15-20 minutes, so as to increase its wear resistance and service life.

6. The method for producing a steel strip for an electric chain saw according to claim 4, characterized in that: The cemented carbide teeth are fixed on the base steel strip by a high temperature welding process, the welding temperature is 800°C-1000°C, the welding time is 5-10 minutes, and the rolling speed of the cold rolling process is 2m / min-5m / min.

7. The method for producing a steel strip for an electric chain saw according to claim 4, characterized in that: The etching process is carried out using an acidic solution, the etching time is 10-15 minutes, and the pressure of the sintering process is 100MPa-200MPa.

8. The method for producing a steel strip for an electric chain saw according to claim 4, characterized in that: The pressure of the hot pressing process is 5MPa-10MPa.