Periodically antibacterial composite magnesium alloy material and preparation method and application thereof

By alternately stacking and high-temperature rolling of magnesium-zinc alloy and magnesium-copper alloy sheets, periodic antibacterial composite magnesium alloy materials are formed, which solves the problems of poor mechanical properties and slow degradation rate of magnesium-copper alloys, and achieves high performance and antibacteriality of bone repair materials Effect.

CN118876559AActive Publication Date: 2024-11-01CHANGSHU MICROTUBE TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410956179.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Medical magnesium-copper alloys have poor mechanical properties and slow corrosion degradation rates, making it difficult to meet the needs of bone repair.

Method used

By alternately stacking and magnesium-zinc alloy sheets and magnesium-copper alloy sheets, and multiple high-temperature rolling and folding, a periodic antibacterial composite magnesium alloy material is formed, and the magnesium-copper alloy is modified using the mechanical properties of magnesium-zinc alloy, and the magnesium-copper alloy is modified through The alternating release of zinc ions and copper ions regulates the degradation rate and achieves antibacterial effects.

Benefits of technology

It significantly improves the mechanical properties and degradation properties of composite magnesium alloy materials, achieves excellent antibacterial effects, and is suitable for bone repair materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876559A_ABST
    Figure CN118876559A_ABST
Patent Text Reader

Abstract

The invention provides a periodic antibacterial composite magnesium alloy material and a preparation method and application thereof, and belongs to the technical field of alloy materials. The magnesium-zinc alloy plates and the magnesium-copper alloy plates are alternately stacked, and the composite magnesium alloy material with multiple layers of magnesium-zinc alloy layers and multiple layers of magnesium-copper alloy layers alternately arranged can be obtained in a multi-time rolling-folding-rolling mode. The magnesium-zinc alloy and the magnesium-copper alloy layer are alternately distributed, on one hand, the magnesium-copper alloy can be modified through the good mechanical property of the magnesium-zinc alloy, and the defect that the mechanical property of the magnesium-copper alloy is poor is overcome; and on the other hand, the magnesium-zinc alloy layers and the magnesium-copper alloy layers which are alternately arranged can achieve alternate interval release of zinc ions and copper ions, the degradation rate of the composite magnesium alloy can be regulated and controlled, the periodic antibacterial effect can be achieved through intermittent release of the copper ions, and the obtained composite magnesium alloy material is excellent in antibacterial performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and in particular to a periodically antibacterial composite magnesium alloy material and a preparation method and application thereof. Background Art

[0002] Medical magnesium alloys are known as the third generation of biomedical materials as biodegradable medical materials. Magnesium is a mild element to the human body, with good absorbability and biocompatibility. In orthopedic implants, it has a density and elastic modulus close to that of bones. Medical magnesium alloys also have a controllable corrosion rate and have good application prospects in cardiovascular implants and bone repair.

[0003] Copper is an important trace element in human tissues, regulating the metabolism of the human body and the functions of various enzymes. In addition, copper ions have good antibacterial effects. Introducing copper metal into magnesium alloys can give magnesium alloys good antibacterial properties. However, the mechanical properties of magnesium-copper alloys are far inferior to those of common magnesium alloy medical materials, and the corrosion degradation rate is slow, which makes it difficult to meet the actual needs of bone repair, which limits its actual use. Summary of the invention

[0004] In view of this, the present invention aims to provide a periodically antibacterial composite magnesium alloy material and its preparation method and application. The mechanical and degradation properties of the composite magnesium alloy material provided by the present invention are significantly higher than those of magnesium-copper alloy, and the antibacterial effect is achieved through the intermittent release of copper ions.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a periodically antibacterial composite magnesium alloy material, comprising the following steps:

[0007] The magnesium-zinc alloy plate and the magnesium-copper alloy plate are alternately stacked to obtain a plurality of stacked plates; the zinc content of the magnesium-zinc alloy plate is 0.5-2wt%; the copper content of the magnesium-copper alloy plate is 0.1-0.4wt%;

[0008] Performing a first high-temperature rolling on the stacked plurality of plates to obtain a first composite plate;

[0009] The first composite plate is folded in half, and the folded plate is subjected to a second high-temperature rolling to obtain a second composite plate, ... and the steps of folding in half and high-temperature rolling are repeated multiple times to obtain a periodically antibacterial composite magnesium alloy material.

[0010] Preferably, the number of layers of the stacked plurality of plates is 2 to 8.

[0011] Preferably, the thickness of a single magnesium-zinc alloy sheet is 0.1 to 2 mm;

[0012] The thickness of a single magnesium-copper alloy sheet is 0.1 to 2 mm.

[0013] Preferably, the temperature of each high temperature rolling is 100-300°C.

[0014] Preferably, the deformation amount of each high temperature rolling pass is 10 to 90%.

[0015] Preferably, the folding and high-temperature rolling are repeated 2 to 6 times.

[0016] The present invention provides a periodic antibacterial composite magnesium alloy material prepared by the above preparation method, comprising alternately stacked magnesium-zinc alloy layers and magnesium-copper alloy layers;

[0017] The number of the magnesium-zinc alloy layer and the magnesium-copper alloy layer is 10 to 100 in total.

[0018] Preferably, the thickness of the periodic antibacterial composite magnesium alloy material is 0.2-2 mm.

[0019] The present invention provides application of the above-mentioned periodic antibacterial composite magnesium alloy material in the preparation of bone repair materials.

[0020] The present invention provides a method for preparing a composite magnesium alloy material with periodic antibacterial properties, comprising the following steps: alternately stacking a magnesium-zinc alloy sheet and a magnesium-copper alloy sheet to obtain a plurality of stacked sheets; the zinc content of the magnesium-zinc alloy sheet is 0.5-2wt%; the copper content of the magnesium-copper alloy sheet is 0.1-0.4wt%; the stacked sheets are subjected to a first high-temperature rolling to obtain a first composite sheet; the first composite sheet is folded in half, and the folded sheet is subjected to a second high-temperature rolling to obtain a second composite sheet, ... and the steps of folding in half and high-temperature rolling are repeated multiple times to obtain a composite magnesium alloy material with periodic antibacterial properties. The present invention can obtain a composite magnesium alloy material with multiple layers of magnesium-zinc alloy and magnesium-copper alloy layers alternately arranged by alternately stacking magnesium-zinc alloy sheets and magnesium-copper alloy sheets through multiple rolling-folding-rolling methods. The present invention can modify the magnesium-copper alloy by utilizing the good mechanical properties of the magnesium-zinc alloy to solve the defect of poor mechanical properties of the magnesium-copper alloy by alternately distributing the magnesium-zinc alloy and the magnesium-copper alloy layers. On the other hand, the alternating magnesium-zinc alloy layers and magnesium-copper alloy layers can achieve the alternating release of zinc ions and copper ions, which can not only regulate the degradation rate of the composite magnesium alloy, but also achieve a periodic antibacterial effect through the intermittent release of copper ions. The resulting composite magnesium alloy material has excellent antibacterial properties.

[0021] The present invention provides a method for preparing the above-mentioned periodic antibacterial composite magnesium alloy material. The method is simple to operate, low in cost, and easy to realize industrialized mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of the structure of a composite magnesium alloy material with periodic antibacterial properties;

[0023] Figure 2 This is a cross-sectional metallographic image of the periodically antibacterial composite magnesium alloy plate of Example 1;

[0024] Figure 3 This is a cross-sectional metallographic image of the periodically antibacterial composite magnesium alloy plate of Example 2;

[0025] Figure 4 The change of pH value of the composite magnesium alloy plate of Example 2 after being immersed in cast Mg-0.2Cu for 2 weeks;

[0026] Figure 5 The change in pH value of the composite magnesium alloy plate of Example 1 after being immersed in rolled Mg-0.2Cu for 2 weeks. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a periodically antibacterial composite magnesium alloy material, comprising the following steps:

[0028] The magnesium-zinc alloy plate and the magnesium-copper alloy plate are alternately stacked to obtain a plurality of stacked plates; the zinc content of the magnesium-zinc alloy plate is 0.5-2wt%; the copper content of the magnesium-copper alloy plate is 0.1-0.4wt%;

[0029] Performing a first high-temperature rolling on the stacked plurality of plates to obtain a first composite plate;

[0030] The first composite plate is folded in half, and the folded plate is subjected to a second high-temperature rolling to obtain a second composite plate, ... and the steps of folding in half and high-temperature rolling are repeated multiple times to obtain a periodically antibacterial composite magnesium alloy material.

[0031] The present invention alternately stacks the magnesium-zinc alloy sheet and the magnesium-copper alloy sheet to obtain a plurality of stacked sheets. In the present invention, the zinc content of the magnesium-zinc alloy sheet is 0.5-2wt%, preferably 0.8-1.8wt%, more preferably 1-1.5wt%, and the balance is magnesium. In the present invention, the thickness of a single magnesium-zinc alloy sheet is preferably 0.1-2mm, more preferably 0.5-1mm.

[0032] In the present invention, the copper content of the magnesium-copper alloy plate is 0.1-0.4wt%, preferably 0.2-0.3wt%. In the present invention, the thickness of a single magnesium-copper alloy plate is preferably 0.1-2mm, more preferably 0.5-1mm.

[0033] The present invention preferably pre-treats the magnesium-zinc alloy sheet and the magnesium-copper alloy sheet, and the pre-treatment preferably includes grinding, polishing, cleaning and drying in sequence. In the present invention, the grinding method is preferably to grind the surface from coarse to fine with sandpaper until there is no oxide scale on the surface; the polishing method is preferably to use a solution of phosphoric acid + ethylene glycol to chemically polish the magnesium-zinc alloy sheet at 55±5°C, and the volume ratio of phosphoric acid and ethylene glycol is preferably 2:3; in the present invention, the detergent used for cleaning is preferably ethanol, purified water, ethanol and ethanol solution, the cleaning is preferably ultrasonic cleaning, and the number of cleanings is multiple times; the present invention prevents polishing liquid residue by the multiple cleanings; in the present invention, the drying is preferably oven drying.

[0034] In the present invention, the number of layers of the stacked plurality of plates is 2 to 8 layers, preferably 3 to 5 layers.

[0035] After obtaining the stacked multiple plates, the present invention performs a first high-temperature rolling on the stacked multiple plates to obtain a first composite plate. In the present invention, the temperature of the first high-temperature rolling is preferably 100 to 300°C, more preferably 150 to 250°C, and further preferably 200°C. In the present invention, the deformation amount of the first high-temperature rolling pass is preferably 10 to 90%, more preferably 30 to 60%.

[0036] After obtaining the first composite sheet, the present invention folds the first composite sheet in half, and performs a second high-temperature rolling on the folded sheet to obtain a second composite sheet, ... and repeats the steps of folding in half and high-temperature rolling multiple times to obtain a composite magnesium alloy material with periodic antibacterial properties. In the present invention, the folding method is preferably folding along the center line. The present invention doubles the number of layers of the composite sheet by folding in half.

[0037] In the present invention, the temperature of the second high temperature rolling is preferably 100-300° C., more preferably 150-250° C., and further preferably 200° C. In the present invention, the deformation amount of the second high temperature rolling is preferably 10-90%, and more preferably 30-60%.

[0038] In the present invention, the folding and high temperature rolling are repeated preferably 2 to 6 times, more preferably 3 to 5 times. In the present invention, the temperature of each high temperature rolling is preferably 100 to 300°C, more preferably 150 to 250°C, and further preferably 200°C; the deformation per pass is preferably 10 to 90%, more preferably 30 to 60%.

[0039] The present invention provides a periodic antibacterial composite magnesium alloy material prepared by the above preparation method, comprising alternately stacked magnesium-zinc alloy layers and magnesium-copper alloy layers;

[0040] The number of the magnesium-zinc alloy layer and the magnesium-copper alloy layer is 10 to 100 layers in total, preferably 20 to 80 layers, and more preferably 30 to 50 layers.

[0041] In the present invention, the thickness of the periodically antibacterial composite magnesium alloy material is preferably 0.2 to 2 mm, more preferably 0.5 to 1.5 mm, and further preferably 0.8 to 1.2 mm.

[0042] In the present invention, the thickness of the single-layer magnesium-zinc alloy layer and the magnesium-copper alloy layer is preferably 4 to 40 μm, more preferably 10 to 30 μm, independently.

[0043] In the present invention, the structural schematic diagram of the periodic antibacterial composite magnesium alloy material is as follows Figure 1 shown.

[0044] The present invention provides the use of the above-mentioned periodic antibacterial composite magnesium alloy material in the preparation of bone repair materials. In the present invention, the periodic antibacterial composite magnesium alloy material is preferably a bone plate material.

[0045] The periodic antibacterial composite magnesium alloy material provided by the present invention, its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0046] Example 1

[0047] Two magnesium-zinc alloy plates with a zinc content of 1 wt% and two magnesium-copper alloy plates with a copper content of 0.2 wt%, each with a thickness of 2 mm, were prepared. The magnesium-zinc alloy plates and the magnesium-copper alloy plates were ground, polished, cleaned and dried to remove the oxide layer on the surface of the plates.

[0048] The above magnesium-zinc alloy sheet and magnesium-copper alloy sheet are alternately stacked, and the alternately stacked multilayer sheet is subjected to the first high-temperature rolling (4 layers) at a temperature of 300°C and a deformation of 60% per pass, and then folded in half, and the folded sheet is subjected to the second high-temperature rolling (8 layers) at a temperature of 300°C and a deformation of 60% per pass, and folded in half again, and the folded sheet is subjected to the third high-temperature rolling (16 layers) at a temperature of 300°C and a deformation of 40% per pass, to obtain a periodically antibacterial composite magnesium alloy sheet, including alternately stacked high-purity magnesium layers and magnesium-zinc alloy layers, with a total of 16 layers, a final thickness of 1.2 mm, and an average single-layer thickness of 0.075 mm. After mechanical testing, the material has a tensile strength of 153 MPa.

[0049] Figure 2 This is a cross-sectional metallographic image of the periodic antibacterial composite magnesium alloy plate of Example 1 (scale is 100 μm). It can be seen that the entire material cross section is clearly layered and different layers are well fused.

[0050] Example 2

[0051] Four magnesium-zinc alloy plates with a zinc content of 1 wt% and four magnesium-copper alloy plates with a copper content of 0.2 wt%, each with a thickness of 2 mm, were prepared. The magnesium-zinc alloy plates and magnesium-copper alloy plates were ground, polished, cleaned and dried to remove the oxide layer on the surface of the plates.

[0052] The above magnesium-zinc alloy sheet and magnesium-copper alloy sheet are alternately stacked, and the alternately stacked multilayer sheet is subjected to the first high-temperature rolling (8 layers) at a temperature of 300°C and a deformation of 60% per pass, and then folded in half, and the folded sheet is subjected to the second high-temperature rolling (16 layers) at a temperature of 300°C and a deformation of 60% per pass, and folded in half again, and the folded sheet is subjected to the third high-temperature rolling (32 layers) at a temperature of 300°C and a deformation of 60% per pass, to obtain a periodically antibacterial composite magnesium alloy sheet, including alternately stacked high-purity magnesium layers and magnesium-zinc alloy layers, with a total number of 32 layers, a final thickness of 1.9 mm, and an average single-layer thickness of 0.06 mm. After mechanical testing, the material has a tensile strength of 160 MPa.

[0053] Figure 3 This is a cross-sectional metallographic image of the periodically antibacterial composite magnesium alloy plate of Example 2 (scale is 100 μm). It can be seen that the entire material cross section is clearly layered and the different layers are well fused.

[0054] Comparative Example 1

[0055] A 2 mm cast magnesium-copper alloy plate (referred to as cast Mg-0.2Cu) with a copper content of 0.2 wt% was prepared for comparison with Example 2. The tensile strength of the alloy was 60 MPa, which was significantly lower than the mechanical properties of the materials in Examples 1 and 2.

[0056] Figure 4 The changes in pH value after corrosion of the composite magnesium alloy plate of Example 2 and cast Mg-0.2Cu were immersed in 200 mL of PBS solution for 2 weeks. It can be seen that the corrosion rate of cast Mg-0.2Cu was faster than that of antibacterial material in the first 7 days, and the corrosion rate slowed down in the later period as the material was dissolved. The composite magnesium alloy plate of Example 2 showed a significant decrease after 14 days, indicating that the corrosion rate of Example 2 was longer than that of cast Mg-0.2Cu.

[0057] Comparative Example 2

[0058] Two 2mm magnesium-copper alloy plates with a copper content of 0.2wt% were laminated and rolled at high temperature using a twin-roll mill at a temperature of 300°C and a deformation of 60% per pass to obtain a magnesium-copper alloy plate material with a thickness of 1.8mm (hereinafter referred to as rolled Mg-0.2Cu), which was compared with Example 1. The tensile strength of the alloy was 116MPa, which was significantly lower than the mechanical properties of the materials in Examples 1 and 2.

[0059] Figure 5 The figure shows the change in pH value after corrosion of the composite magnesium alloy plate of Example 1 and rolled Mg-0.2Cu in 200 mL of PBS solution for 2 weeks. It can be seen that the corrosion rate of rolled Mg-0.2Cu is faster than that of the antibacterial material in the first 4 days, and the corrosion rate slows down in the later period as the material is ablated; while the composite magnesium alloy plate of Example 1 has a significant decrease after 14 days, indicating that the corrosion rate of Example 1 can support a much longer time than that of rolled Mg-0.2Cu.

[0060] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a periodically antibacterial composite magnesium alloy material, comprising the following steps: The magnesium-zinc alloy plate and the magnesium-copper alloy plate are alternately stacked to obtain a plurality of stacked plates; the zinc content of the magnesium-zinc alloy plate is 0.5-2wt%; the copper content of the magnesium-copper alloy plate is 0.1-0.4wt%; Performing a first high-temperature rolling on the stacked plurality of plates to obtain a first composite plate; The first composite plate is folded in half, and the folded plate is subjected to a second high-temperature rolling to obtain a second composite plate, ... and the steps of folding in half and high-temperature rolling are repeated multiple times to obtain a periodically antibacterial composite magnesium alloy material.

2. The preparation method according to claim 1, characterized in that: The number of layers of the stacked multiple plates is 2 to 8.

3. The preparation method according to claim 1, characterized in that: The thickness of a single magnesium-zinc alloy sheet is 0.1 to 2 mm; The thickness of a single magnesium-copper alloy sheet is 0.1 to 2 mm.

4. The preparation method according to claim 1, characterized in that: The temperature of each high temperature rolling is 100-300°C.

5. The preparation method according to claim 1 or 4, characterized in that: The deformation amount of each high temperature rolling pass is 10 to 90%.

6. The preparation method according to claim 1, characterized in that: The folding and high temperature rolling are repeated 2 to 6 times.

7. The periodic antibacterial composite magnesium alloy material prepared by the preparation method according to any one of claims 1 to 6 comprises alternately stacked magnesium-zinc alloy layers and magnesium-copper alloy layers; The number of the magnesium-zinc alloy layer and the magnesium-copper alloy layer is 10 to 100 in total.

8. The periodic antibacterial composite magnesium alloy material according to claim 7, characterized in that: The thickness of the periodically antibacterial composite magnesium alloy material is 0.2-2 mm.

9. Use of the periodically antibacterial composite magnesium alloy material according to claim 7 or 8 in the preparation of bone repair materials.

Citation Information

Patent Citations

  • Degradable multi-layer Mg / Zn composite material for medical use and preparation method thereof

    CN111450322A

  • Alloy material with antibacterial property and high toughness and preparation method and application thereof

    CN112371983A

  • Layered special-shaped texture magnesium alloy and preparation method thereof

    CN114535341A