Application of ammonium fluoride as activating agent and alkyl amide as collecting agent in copper oxide ore flotation and flotation method

By using ammonium fluoride and alkyl amide as activators and collectors in copper oxide flotation, the problem of low recovery rate of silica malachite is solved, and high-efficiency and low-cost copper oxide is achieved. Resource recycling.

CN119034949APending Publication Date: 2024-11-29HUNAN RES INST FOR NONFERROUS METALS CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411279190.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Among the existing copper oxide flotation technology, the vulcanization-yellowicide method has a low recovery rate of silica malachite, complex process and high cost. Traditional agents consume a lot, making it difficult to effectively develop and utilize copper oxide resources.

Method used

Ammonium fluoride is used as the activator and alkyl amide as the collector, and flotation is performed directly through ionization and chelation reactions, which significantly improves the recovery rate of malachite, reduces agent consumption, and simplifies the process flow.

Benefits of technology

It realizes efficient recycling of malachite, with a 2-3-fold increase in recovery rate, reduces drug consumption, simple process, low cost, and no need for vulcanizing agents, providing a green and economical flotation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034949A_ABST
    Figure CN119034949A_ABST
Patent Text Reader

Abstract

The invention provides application of ammonium fluoride as an activating agent and alkyl amide as a collecting agent in copper oxide ore flotation and a flotation method, and relates to the technical field of copper oxide ore flotation. According to the method, ammonium fluoride is adopted for directionally activating the silicon malachite, hexylamide and copper ions generate a two-tooth chelation collecting agent, the flotation selectivity can be effectively enhanced, and the grade and the recovery rate of the silicon malachite are improved. The method has the advantages of simple process, low cost, low medicament consumption, high mineralization speed (without adding a vulcanizing agent to vulcanize the surface of the silicon malachite) and high recovery rate, and can obviously improve the recovery rate of the silicon malachite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flotation of copper oxide ores, and in particular to the application of ammonium fluoride as an activator and alkylamide as a collector in flotation of copper oxide ores and a flotation method. Background Art

[0002] With the continuous reduction of easy-to-select copper sulfide ore resources, people have begun to turn their attention to the more difficult-to-select copper oxide ore resources. Copper oxide ore resources account for 25-30% of all copper ore resources, but copper ore resources with industrial value account for a small proportion, only about 10% of all copper ore resources. Therefore, the rational development and utilization of copper oxide ore resources has become an important research direction for mineral processing.

[0003] Bound copper oxide is a general term for a class of substances. It is a state of existence of copper oxide minerals in ores. Bound copper oxide exists in copper oxide ores and copper ores. The separation and recovery of bound copper oxide has always been a research hotspot and a difficulty in mineral flotation separation. It is called "unselectable copper ore". Research on the recovery and utilization of bound copper oxide is of great significance for improving the efficient and comprehensive utilization of copper resources. Bound copper oxide has been regarded as an unselectable mineral for many years. Since the diffusion ability of cyanide is weaker than that of other ions, it cannot dissolve the bound copper oxide wrapped in the gangue. Therefore, cyanide cannot leach copper oxide, which is called bound copper oxide. Commonly used copper oxide mineral activators such as sodium sulfide and collectors such as xanthate, hydroxamic acid, and black medicine cannot select bound copper oxide. However, through in-depth and systematic research in recent years, it has been found that bound copper oxide can be sorted.

[0004] Chrysocolla is a copper-containing silicate mineral with the chemical formula (Cu, Al) 2 H 2 Si 2 O 5 (OH)·nH 2 O, mainly produced in the oxidation zone of copper-bearing deposits, belongs to the combined oxide copper ore, often with malachite (copper carbonate), azurite (copper carbonate), cuprite (copper oxide), natural copper symbiosis. In addition, it often appears together with chalcedony, which is an important inclusion of some blue or green chalcedony.

[0005] Most of the oxidized copper ores have problems such as high mudification, poor floatability, complex ore properties, and low flotation recovery. In particular, chrysocolla is a bound copper mineral. The copper in chrysocolla is wrapped by silicate and hydroxyl groups, which hinders the interaction between the sulfiding agent and the collector and the chrysocolla, resulting in low sulfide hydrophobicity efficiency. The traditional sulfide-flotation chrysocolla recovery rate is extremely low, and its recovery rate is usually 20% to 40%. In recent years, due to the decreasing resources of easy-to-select sulfide copper ores, the development and utilization of difficult-to-select oxidized copper ores has attracted more and more attention. In addition to the sulfide-xanthate method, the beneficiation of oxidized copper ores has also seen the emergence of chelate flotation, chemical beneficiation, microwave irradiation flotation, hydrothermal sulfidation flotation, and ammonia leaching sulfidation precipitation flotation. These methods have common defects such as low recovery, heavy pollution, large investment, or high cost.

[0006] With the reduction of copper sulfide minerals, more and more people have turned their attention to the recovery of copper oxide mineral resources. The traditional flotation of copper oxide is the sulfide-xanthate flotation method, that is, first use a sulfiding agent such as sodium sulfide or sodium hydrogen sulfide to sulfide the surface of the copper oxide to form a hydrophobic copper sulfide film, and then use hydroxamic acid and xanthate collectors to float the copper oxide. Although it has a good effect on copper oxide ores such as malachite, chrysocolla is wrapped by silicate and hydroxyl groups, making sulfidation and flotation difficult, resulting in serious waste of chrysocolla resources. Therefore, there is an urgent need for a flotation method and an efficient flotation agent that can further improve the recovery rate. Summary of the invention

[0007] The invention provides application of ammonium fluoride as an activator and alkylamide as a collector in flotation of copper oxide ore and a flotation method, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0008] In order to achieve the above-mentioned purpose, based on the method research of the mineral structure of chrysocolla and the action mechanism of new flotation reagents, the embodiments of the present invention provide the application of ammonium fluoride as an activator and an alkylamide as a collector in the flotation of copper oxide ore and a flotation method. The method has the advantages of simple process, low cost, low reagent consumption, fast mineralization speed (no need to add a sulfiding agent to sulfide the surface of chrysocolla), high recovery rate, and can significantly improve the recovery rate of chrysocolla.

[0009] One purpose of the embodiments of the present invention is to provide the use of ammonium fluoride as an activator and alkylamide as a collector in the flotation of copper oxide ore, wherein the carbon number of the alkyl group in the alkylamide is 4 to 8.

[0010] According to one aspect of an embodiment of the present invention, the alkyl amide is at least one of hexyl amide, pentyl amide and butyl amide.

[0011] According to one aspect of an embodiment of the present invention, the copper oxide ore is chrysocolla, malachite, azurite, or cuprite.

[0012] According to one aspect of an embodiment of the present invention, ammonium fluoride and alkylamide selectively float chrysocolla.

[0013] Another object of an embodiment of the present invention is to provide a flotation method, comprising the following steps:

[0014] S1: taking chrysocolla ore, crushing, grinding and screening to obtain ore powder;

[0015] S2: adding the ore powder and water into the flotation tank, stirring, and adding the above-mentioned activator for activation;

[0016] S3: adding the above-mentioned collector for chelation;

[0017] S4: adding a frother for flotation to obtain chrysocolla concentrate.

[0018] According to one aspect of an embodiment of the present invention, the ore powder has a fineness of 40% to 90% of -200 mesh.

[0019] According to one aspect of the embodiment of the present invention, the usage of ammonium fluoride is 30-100 mg / L.

[0020] According to one aspect of the embodiments of the present invention, the amount of the collector is 80-150 mg / L.

[0021] According to one aspect of an embodiment of the present invention, the mass ratio of the collector to ammonium fluoride is (1-3): 1. Preferably, the mass ratio of the collector to ammonium fluoride is 2:1.

[0022] According to one aspect of the embodiment of the present invention, the foaming agent is 2 # Any one of oil, ether alcohol, methyl isobutyl carbinol (MIBC), the dosage is 5-60 mg / L. Preferably, the dosage of the foaming agent is 20 mg / L.

[0023] mechanism

[0024] Ammonium fluoride ionizes to produce fluoride ions and ammonium ions. The fluoride ions will dissolve the silicate at the interface of chrysocolla, exposing more active copper ions. The chemical reaction of fluoride ion corrosion and dissolution of silicate is shown in the following chemical reaction formula (1);

[0025] 6F - +SiO 3 2- +H + →SiF 6 2- +H 2 O (1)

[0026] Ammonium ions coordinate with copper in chrysocolla, destroying the hydration film on the surface of chrysocolla, changing the electrical properties and hydrophilicity of chrysocolla, and providing more active sites for the collector to directionally activate chrysocolla, thereby producing selective directionally activated chrysocolla.

[0027] Under the action of ammonium fluoride, the acyl and amine groups in the collector hexylamide form a ring-shaped chelate with the copper on the surface of siliceous malachite (as shown in the following structural diagram), making the siliceous malachite hydrophobic. This ring-shaped chelation is a chemical adsorption, and its adsorption stability is much greater than the electrostatic physical adsorption of amines. It does not adsorb quartz and calcium carbonate, thereby achieving selective flotation of siliceous malachite.

[0028]

[0029] The above scheme of the present invention has the following beneficial effects:

[0030] (1) The directional activation-chelating capture flotation method of the present invention does not require the use of a sulfiding agent for sulfidation. Under the directional activation of ammonium fluoride, hexylamide is directly added to float the siliceous malachite. Compared with the existing sulfidation-flotation method, a soluble sulfiding agent must be used to add sodium sulfide or sodium hydrogen sulfide to pre-sulfidize the copper oxide mineral. The sulfiding agent consumes 2-4 kg / t. After sufficient stirring, a collector such as xanthate, black medicine, etc. is used to float the sulfided copper oxide mineral. The collector consumes 1-2 kg / t. Usually, the sulfiding agent is unstable and easy to fall off during sulfidation. The sulfiding agent must be added continuously in batches. In short, the process is complicated and cumbersome. In addition, in the existing conventional flotation method of siliceous malachite, a sulfiding agent is usually added for sulfidation. However, since the copper in siliceous malachite is wrapped by silicate and hydroxyl groups, it is difficult to form a copper sulfide film with the surface of siliceous malachite. The flotation effect is extremely poor and the recovery rate is very low.

[0031] (2) The present invention uses ammonium fluoride to directionally activate chrysocolla, and hexylamide and copper ions produce a two-tooth chelating collector, which effectively enhances the selectivity of flotation and improves the grade and recovery rate of chrysocolla.

[0032] (3) The flotation method of the present invention not only requires less flotation reagent, but also consumes 0.6-0.8 kg / t of activator and 0.8-1.3 kg / t of collector, compared with the conventional sulfidation-flotation method, which consumes 2-4 kg / t of sulfiding agent and 1-2 kg / t of collector, and the total flotation reagent consumption is reduced by 2-3 times. The method also has strong capture power and good selectivity for siliceous malachite. Moreover, the reagents used are all sulfide-free and relatively safe, which provides a new approach, new method and new reagent for green and economic flotation recovery of siliceous malachite. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 is a schematic flow chart of a flotation method according to an embodiment of the present invention;

[0035] Figure 2 is a comparison chart of flotation results of Example 1 of the present invention;

[0036] Figure 3 is a comparison diagram of flotation results of Example 2 of the present invention;

[0037] Figure 4 is a comparison diagram of flotation results of Example 3 of the present invention;

[0038] Figure 5 is a comparison diagram of flotation results of Example 4 of the present invention;

[0039] Figure 6 is a comparison chart of flotation results of Example 5 of the present invention;

[0040] Figure 7 is a comparison diagram of flotation results of Example 6 of the present invention;

[0041] Figure 8 It is a schematic flow chart of the flotation method of Example 6 of the present invention. DETAILED DESCRIPTION

[0042] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0043] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0044] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0045] In view of the existing problems, the present invention provides the application of ammonium fluoride as an activator and alkylamide as a collector in the flotation of copper oxide ore, wherein the carbon number of the alkyl group in the alkylamide is 4-8.

[0046] According to one aspect of an embodiment of the present invention, the alkyl amide is at least one of hexyl amide, pentyl amide and butyl amide.

[0047] According to one aspect of an embodiment of the present invention, the copper oxide ore is chrysocolla, malachite, azurite, or cuprite.

[0048] According to one aspect of an embodiment of the present invention, ammonium fluoride and alkylamide selectively float chrysocolla.

[0049] Another object of the embodiment of the present invention is to provide a flotation method, the flotation process diagram is as follows Figure 1 As shown, the following steps are included:

[0050] S1: taking chrysocolla ore, crushing, grinding and screening to obtain ore powder;

[0051] S2: adding the ore powder and water into the flotation tank, stirring, and adding the above-mentioned activator for activation;

[0052] S3: adding the above-mentioned collector for chelation;

[0053] S4: adding a frother for flotation to obtain chrysocolla concentrate.

[0054] According to one aspect of an embodiment of the present invention, the ore powder has a fineness of 40% to 90% of -200 mesh.

[0055] According to one aspect of the embodiment of the present invention, the usage of ammonium fluoride is 30-100 mg / L.

[0056] According to one aspect of the embodiments of the present invention, the amount of the collector is 80-150 mg / L.

[0057] According to one aspect of an embodiment of the present invention, the mass ratio of the collector to ammonium fluoride is (1-3):1. Preferably, the mass ratio of the collector to ammonium fluoride is 2:1.

[0058] According to one aspect of the embodiment of the present invention, the foaming agent is 2 # Any one of oil, ether alcohol, methyl isobutyl carbinol (MIBC), the dosage is 5-60 mg / L. Preferably, the dosage of the foaming agent is 20 mg / L.

[0059] The directional activation-chelating capture flotation method of the present invention does not need to use a sulfiding agent for sulfidation. Under the directional activation of ammonium fluoride, hexylamide is directly added to float the siliceous malachite. Compared with the existing sulfidation-flotation method, a soluble sulfiding agent must be used to add sodium sulfide or sodium hydrogen sulfide to pre-sulfidize the copper oxide mineral. The sulfiding agent consumes 2-4kg / t. After sufficient stirring, the collector of the sulfide ore, such as yellow medicine, black medicine, etc., is used to float the sulfided copper oxide mineral. The collector consumes 1-2kg / t. Usually, the sulfiding agent is unstable and easy to fall off during sulfidation. The sulfiding agent must be continuously added in batches. In short, the process is complicated and cumbersome. In addition, a sulfiding agent is usually added in the existing conventional flotation method of siliceous malachite for sulfidation. However, since the siliceous malachite copper is wrapped by silicate and hydroxyl, it is difficult to form a copper sulfide film with the surface of the siliceous malachite, and the flotation effect is extremely poor, and the recovery rate is very low.

[0060] The following is a detailed description with reference to specific embodiments.

[0061] Example 1

[0062] This embodiment provides a flotation method.

[0063] The method of this embodiment specifically includes the following steps:

[0064] The sample used in the test is pure chrysocolla mineral. After crushing, grinding and screening, a -200 mesh chrysocolla powder sample was obtained. 10g of 90% -200 mesh chrysocolla and 100mL of water were added to a 150mL flotation tank. Flotation tests were conducted with hexylamide, butylamide and heptylamide. Three parallel tests were designed. First, an equal amount of ammonium fluoride 50mg / L was added, stirred for 1min, and then butylamide 80mg / L was added, stirred for 1min, and a foaming agent 2 was added. # (20mg / L), stir for 1min, then flotation, the scraping time is 3min; ② Hexylamide 80mg / L, stir for 1min, add frother 2 # (20mg / L), stir for 1min, then flotation, the scraping time is 3min; ③ Heptyl amide 80mg / L, stir for 1min, add frother 2 # (20mg / L), stirred for 1min, and then flotation was performed, and the scraping time was 3min; the test process is as follows Figure 1 The test results are shown in Figure 2 As shown, the recovery rate of butyl amide is 78.3%, the recovery rate of hexyl amide is 81.8%, and the recovery rate of heptyl amide is 79.9%, that is, ②>③>①.

[0065] Example 2

[0066] This embodiment provides a flotation method.

[0067] The method of this embodiment specifically includes the following steps:

[0068] The sample used in the test is pure chrysocolla mineral, which is crushed, ground and sieved to obtain a -200 mesh chrysocolla powder sample. Add 10g of 90% -200 mesh chrysocolla and 100mL of water to a 150mL flotation tank, stir for 1min, add different proportions of hexylamide and ammonium fluoride (the mass ratio of hexylamide and ammonium fluoride is about 1:1, 2:1, 3:1 respectively), stir for 1min, add frother 2 # Oil (20mg / L), stirred for 1min, and then flotation was performed, with a frothing time of 3min. Figure 1 The test results are shown in Figure 3 As shown, the recovery rate is highest when the ratio of hexylamide to ammonium fluoride is 2:1.

[0069] Example 3

[0070] This embodiment provides a flotation method.

[0071] The method of this embodiment specifically includes the following steps:

[0072] The sample used in the test is pure chrysocolla mineral, which is crushed and ground into 60%-200 mesh chrysocolla powder sample. Add 10g chrysocolla with a fineness of 60%-200 mesh and 100mL of water to a 150mL flotation tank, stir for 1min, and then add different collectors (the dosage is 80mg / L). Four groups of comparative tests are designed, namely ① xanthate; ② hexylamide; ③ dodecylamine; ④ hexylamide + ammonium fluoride (the mass ratio of hexylamide and ammonium fluoride is 2:1). Stir for 1min, add frother 2 # Oil 20mg / L, stirred for 1min and then scraped for flotation, the scraping time was 3min. The obtained concentrate product was weighed after drying, and the recovery rate was calculated. The test process is as follows Figure 1 The results are shown in Figure 4 As shown, from Figure 4 It can be seen that the recovery rate is ④>②>③>>①. That is to say, hexylamide and ammonium fluoride can significantly improve the recovery rate of chrysocolla.

[0073] Example 4

[0074] This embodiment provides a flotation method.

[0075] The method of this embodiment specifically includes the following steps:

[0076] The sample used in the test is pure mineral malachite, which is crushed, ground and sieved to obtain a malachite powder sample of 70%-200 mesh. Add 10g of 70%-200 mesh malachite and 100mL of water to a 150mL flotation tank, stir for 1min, add the prepared hexylamide collector (hexylamide dosage is 80mg / L), and add 30mg / L of ammonium fluoride (the mass ratio of hexylamide to ammonium fluoride is about 2:1), stir for 1min, and add 20mg / L of frother. # Oil (①0mg, ②20mg / L, ③60mg / L, ④20mg / L without ammonium fluoride), stirred for 1min, and then flotation was performed. The scraping time was 3min. The test results are as follows Figure 5 As shown, from Figure 5 As can be seen, adding 20mg / L2 # The recovery rate of chrysocolla in oil is greater than 80%. However, if ammonium fluoride is not added, 20 mg / L 2 # The recovery of chrysocolla from oil was only 55%, much lower than that achieved by the directional activator ammonium fluoride.

[0077] Example 5

[0078] This embodiment provides a flotation method.

[0079] The method of this embodiment specifically includes the following steps:

[0080] The samples used in the test are pure mineral chrysocolla, quartz and calcium carbonate. After crushing, grinding and screening, powder samples with a fineness of 70%-200 mesh were obtained. The mass ratio of chrysocolla, quartz and calcium carbonate was 1:1:1 to obtain a mixed mineral MX. 10g of mixed mineral MX with a fineness of 70%-200 mesh and 100mL of water were added to a 150mL flotation tank. After stirring for 1 minute, the prepared hexylamide collector (hexylamide dosage is 80mg / L) was added, and at the same time, 30mg / L of ammonium fluoride was added (the mass ratio of hexylamide and ammonium fluoride is about 2:1), stirred for 1 minute, and a frother 2 was added. # Oil 20mg / L, stirred for 1min, and then flotation was performed. The scraping time was 3min. The test results were as follows: Figure 6 As shown, from Figure 6 It can be seen that the recovery rate of chrysocolla reaches 80%, while the recovery rates of quartz and calcium carbonate are 26% and 32% respectively; the content of chrysocolla in copper concentrate is 58%. The test shows that the flotation method has good selectivity.

[0081] Example 6

[0082] This embodiment provides a flotation method.

[0083] The method of this embodiment specifically includes the following steps:

[0084] The sample used in the test is an oxidized copper ore in Africa, whose main components are chalcocite, bornite, malachite, chrysocolla, a small amount of azurite, gangue minerals (quartz, dolomite and calcium carbonate), etc. The oxidation rate is about 70%, the content of chrysocolla in the oxidized copper ore is about 60%, and the content of malachite is about 40%. 1000g of the ore sample was crushed and ground into a 60%-200 mesh slurry sample. The ground sample was floated in a 3L mechanical agitator flotation machine. The operating procedure is: after stirring for 1 minute to adjust the slurry, two groups of comparative tests were designed, first adding xanthate and 2 # Oil flotation copper sulfide ore, the process test is one roughing, two sweeping and two refining closed-loop cycle, to obtain copper sulfide concentrate, and then float copper oxide ore, the flotation process is one roughing, three sweeping and two refining closed-loop cycle, the test process is as follows Figure 7 ① Directed activation-chelation capture flotation test, copper oxide roughing: add 20 mg / L ammonium fluoride, stir for 1 min, add 40 mg / L hexylamide, 2 # The amount of oil used is 20 mg, stirred for 1 min, and scraped for 3 min; Sweep 1: add 10 mg / L of ammonium fluoride, stirred for 1 min, add 20 mg / L of hexylamide, stirred for 1 min, 2 # The oil dosage is 10mg / L, stir for 1min, scrape and foam for 3min; Sweep 2: add ammonium fluoride 10mg / L, stir for 1min, add hexyl amide dosage 15mg / L, 2 # The oil dosage is 10mg / L, stir for 1min, scrape and foam for 3min; Sweep 3: add hexyl amide dosage of 5mg / L, 2 # The oil dosage is 10 mg / L, stirring for 1 min, scraping and foaming for 3 min; copper sulfide concentrate and copper oxide concentrate are obtained. ② Sulfide-flotation recovery of copper oxide ore test, copper oxide roughing: add 50 mg / L sodium sulfide, stir for 1 min, add 50 mg / L butyl xanthate, 2 # The oil dosage is 20mg / L, stir for 1min, scrape and foam for 3min; Sweep 1: add sodium sulfide 40mg / L, stir for 1min, add butyl xanthate dosage 40mg / L, 2 # The oil dosage is 10mg / L, stir for 1min, scrape and foam for 3min; Sweep 2: add 30mg / L sodium sulfide, stir for 1min, add 30mg / L butyl xanthate, 2 # The oil dosage is 10mg / L, stir for 1min, scrape and foam for 3min; Sweep 3: Add butyl xanthate dosage of 15mg / L, 2 # The oil dosage is 10 mg / L, stirring for 1 min, scraping and foaming for 3 min; copper sulfide concentrate and copper oxide concentrate are obtained. Figure 8 The results are shown in Table 1.

[0085] Table 1 Example 5 Test results / %

[0086]

[0087] ① is the flotation process of the present invention, and the recovery rate of chrysocolla is 78.2%, which is much higher than the recovery rate of 31% of chrysocolla in the conventional flotation process ②.

[0088] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Application of ammonium fluoride as activator and alkylamide as collector in flotation of copper oxide ore. It is characterized in that The carbon number of the alkyl group in the alkyl amide is 4 to 8.

2. The use according to claim 1, It is characterized in that The alkyl amide is at least one of hexyl amide, pentyl amide and butyl amide.

3. The use according to claim 1, It is characterized in that The copper oxide ore is chrysocolla, malachite, azurite and cuprite.

4. The use according to claim 1, It is characterized in that Selective flotation of chrysocolla by ammonium fluoride and alkylamide.

5. A flotation method, It is characterized in that The steps include: S1: taking chrysocolla ore, crushing, grinding and screening to obtain ore powder; S2: adding the ore powder and water into the flotation tank, stirring, and adding ammonium fluoride for activation; S3: adding a collector to carry out a chelating reaction; S4: adding a frother for flotation to obtain chrysocolla concentrate.

6. The flotation method according to claim 5, It is characterized in that The ore powder fineness is 40% to 90% of -200 mesh.

7. The flotation method according to claim 5, It is characterized in that The dosage of the ammonium fluoride is 30-100 mg / L.

8. The flotation method according to claim 5, It is characterized in that The dosage of the collector is 80-150 mg / L.

9. The flotation method according to claim 5, It is characterized in that The mass ratio of the collector to ammonium fluoride is (1-3):

1.

10. The flotation method according to claim 5, It is characterized in that The foaming agent is 2 # Oil, dosage is 5-60 mg / L.

Citation Information

Cited By

  • Activation method of silicon malachite mineral and flotation method of high-alkalinity copper oxide ore or copper cobalt oxide ore

    CN119456215A

  • A method of activation of a chrysocolla mineral and a method of flotation of a high-alkaline copper oxide ore or a copper cobalt oxide ore

    CN119456215B