Solvent-free damp-heat-resistant polyaspartic acid ester coating and preparation method thereof

By adding hydrophobically modified cellulose nanocrystals and HDI trimer-loaded silicon-aluminum-based ceramic hollow microbeads to the polyasparticle coating, the swelling problem of polyasparticle coating in humid and heat environments is solved. It achieves better adhesion and moisture and heat resistance, and improves the stability and application scenarios of the coating.

CN118879175AActive Publication Date: 2024-11-01SUZHOU PEIQI MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411114425.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Polyaspartate coatings are prone to swelling and damage in high temperature and humidity environments, resulting in peeling off the interface between the coating and the substrate. It is difficult for the prior art to effectively improve its moisture and heat resistance and application scenarios.

Method used

Using solvent-free combination technology, including polyaspartate, hydrophobically modified cellulose nanocrystals and HDI trimers, through specific dispersants, defoamers, leveling agents, anti-settling agents, light stabilizers The ratio with wetting agent and the loading of HDI trimer on silicon-aluminum-based ceramic hollow microbeads form a uniform and dense coating structure, extending the curing time and improving the moisture and heat resistance of the coating.

Benefits of technology

It significantly improves the moisture and heat resistance of the coating film, reduces moisture infiltration and bubble formation, extends the service life of the coating, and realizes a green and environmentally friendly and efficient curing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993224680000091
    Figure BDA0004993224680000091
Patent Text Reader

Abstract

The invention relates to the field of coatings, and particularly discloses a solvent-free damp-heat-resistant polyaspartic acid ester coating and a preparation method thereof.The solvent-free damp-heat-resistant polyaspartic acid ester coating comprises the following raw materials in parts by weight: a component A: 20-35 parts of polyaspartic acid ester, 0.5-1 part of a dispersing agent, 0.1-0.2 part of a defoaming agent, 0.2-0.4 part of a flatting agent, 0.1-0.2 part of an anti-settling agent, 0.3-0.5 part of a light stabilizer and 0.1-0.3 part of a wetting agent; the component B comprises the following components in parts by weight: 20-25 parts of HDI (hexamethylene diisocyanate) tripolymer. The coating disclosed by the invention is environment-friendly, solvent-free and good in humidity and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coatings, and more specifically, to a solvent-free, moisture-heat-resistant polyaspartic acid ester coating and a preparation method thereof. Background Art

[0002] Polyaspartic acid ester is a low VOC, high solid content, fast-drying primer / topcoat. It can be directly applied to metal surfaces and used in moderately corrosive environments (up to C3, ISO12944-2) to provide a high degree of protection for the substrate. It is green and environmentally friendly and has good protective effects. However, polyurea coatings cure very quickly, and bubbles and fine lines are likely to remain in the coating film after curing. As water enters the interior at high temperatures, the coating film swells and breaks to produce new cavities, further accelerating the diffusion of water in the coating film, and the degree of peeling at the interface between the coating and the substrate increases until the coating fails.

[0003] In order to improve the adhesion effect and flattening and densifying effect of polyaspartic acid ester coatings, the prior art generally adopts substituents of different structures to prepare polyaspartic acid ester derivatives to adjust the curing process of polyaspartic acid ester, but the preparation process is relatively complicated and there is a lot of loss of raw materials. Some people coat the curing agent of polyaspartic acid ester coating with multiple layers to extend the curing time, but the release effect of the curing agent is difficult to control, which easily causes uneven curing, and the protective effect of the obtained coating is unstable after curing. The short trial period, small variety, high cost, and limited moisture and heat resistance of polyaspartic acid ester coatings limit their application scenarios and have not become a mainstream variety. How to provide a solvent-free moisture and heat resistant polyaspartic acid ester coating and its preparation method, and prepare a green and environmentally friendly polyurea coating with good moisture and heat resistance is a problem to be solved. Summary of the invention

[0004] In order to solve the problem of moisture and heat resistance of polyaspartic acid ester coatings, the present application provides a solvent-free moisture and heat resistant polyaspartic acid ester coating and a preparation method thereof.

[0005] In the first aspect, the present application provides a solvent-free, moisture- and heat-resistant polyaspartic acid ester coating, comprising the following raw materials in parts by weight: component A: 20-35 parts of polyaspartic acid ester, 0.5-1 parts of dispersant, 0.1-0.2 parts of defoaming agent, 0.2-0.4 parts of leveling agent, 0.1-0.2 parts of anti-settling agent, 0.3-0.5 parts of light stabilizer, 0.1-0.3 parts of wetting agent, 2-7 parts of hydrophobically modified cellulose nanocrystals, component B: 20-25 parts of HDI trimer.

[0006] The amino group in the molecular structure of polyaspartic acid ester is surrounded by a spatial coronal steric hindrance environment. The special induction effect makes it show a "deceleration" effect in the reaction process with HDI trimer. The curing speed of the obtained coating is reduced, the adhesion to the substrate is better, there are fewer fine lines and bubbles between the coating and the substrate and inside the coating, and water molecules are not easy to penetrate in a hot and humid environment. Adding a certain amount of dispersant, defoamer, leveling agent, anti-settling agent, light stabilizer, and wetting agent makes the coating more evenly and stably dispersed, better adhered to the substrate, and the obtained coating is more uniform and dense. Water vapor is not easy to penetrate in a hot and humid environment. Cellulose nanocrystals are a natural material with a wide range of sources. They are green and environmentally friendly, have high strength and ultra-fine structure, good barrier properties, and high aspect ratio interspersed in the coating to improve the stability of the coating structure. The coating is not easy to deform due to stress when heated, and water molecules are not easy to penetrate. The surface is porous and the structure is loose. The reagents are easy to penetrate in the preparation process, and they can be more closely combined with the rest in the coating, reducing capillary action, and the coating is more resistant to moisture and heat. By hydrophobizing cellulose nanocrystals, the fiber has better dispersion and stability in the coating, and water vapor is not easy to stay on the surface of the coating, and the coating has better resistance to moisture and heat. HDI trimer has low viscosity and good curing effect, which can mix and cure component A more evenly, without solvent, and is green and environmentally friendly.

[0007] In a specific embodiment, the preparation steps of hydrophobically modified cellulose nanocrystals include: adding long-chain silane to ethanol with a volume fraction of 90-95%, ultrasonically treating for 7-12 minutes to obtain a hydrolyzate; adding cellulose nanocrystals to anhydrous ethanol to obtain a mixed solution; dripping the hydrolyzate into the mixed solution, heating at 55-60°C, stirring and refluxing, reacting for 18-19 hours, then cooling, filtering, and vacuum drying to obtain hydrophobically modified cellulose nanocrystals.

[0008] By adopting the above scheme, the preparation process of hydrophobic modification of cellulose nanocrystals is relatively simple and has a high yield. The surface of the prepared hydrophobic modified cellulose nanocrystals has more hydrophobic groups, water vapor is not easy to invade, and the protective effect on the substrate is good.

[0009] In a specific embodiment, the long chain silane is docosenyltriethoxysilane.

[0010] By adopting the above scheme, the surface of the cellulose nanocrystals modified with docosyltriethoxysilane has more hydrophobic groups, water vapor is not easy to stay on the surface of the prepared coating, longer alkane chains are interspersed in the coating, and the hydrophobic groups are mutually associated to form an elastic three-dimensional network structure, which further optimizes the internal structure of the coating, prolongs the path of water vapor invasion, and is not easy to fail in a hot and humid environment. At the same time, it may be that under the action of this silane, the coating structure formed by the components of the present application further causes a certain steric hindrance to polyaspartic acid ester to prolong the curing time. At the same time, the silane structure is not too complicated to prevent polyaspartic acid ester from fully penetrating into the modified cellulose nanocrystals. The applicant found that the coating prepared by modifying cellulose nanocrystals with docosyltriethoxysilane is smoother after curing.

[0011] In a specific embodiment, the HDI trimer of the B component is supported on silica-alumina-based ceramic hollow microspheres.

[0012] By adopting the above scheme, the silicon-aluminum-based ceramic hollow microspheres have a tiny porous hollow structure inside, a fiber hollow mesh structure on the surface, a small particle size, a large surface area, and a surface mesh structure with physical cross-linking points and macromolecular chains that are easy to absorb resin. By adding a certain mass of silicon-aluminum-based ceramic hollow microspheres, the surface of the obtained coating is denser, the load distribution is more uniform, and it has a certain heat insulation effect. The coating is not easy to deform and produce structural defects under the heating state, and the water vapor penetration under hot and humid conditions is avoided. The obtained coating has better resistance to heat and humidity. By loading HDI trimer on silicon-aluminum-based ceramic hollow microspheres, HDI trimer is adsorbed in the mesh structure on the surface of silicon-aluminum-based ceramic hollow microspheres, reducing the reaction rate of HDI trimer and polyaspartic acid ester, prolonging the curing time of the coating, and the obtained coating is smoother and denser.

[0013] In a specific embodiment, the silica-alumina-based ceramic hollow microspheres are n-dodecyltriethoxysilane-modified silica-alumina-based ceramic hollow microspheres.

[0014] By adopting the above scheme, the silicon-aluminum-based ceramic hollow microspheres are modified with n-dodecyltriethoxysilane, the microspheres have better dispersibility in the coating and better compatibility with component A. After the n-dodecyltriethoxysilane-modified silicon-aluminum-based ceramic hollow microspheres are added to component A, the long chain of n-dodecyltriethoxysilane and docosenetriethoxysilane are intertwined to a certain extent, and the obtained coating film is denser.

[0015] In a specific embodiment, the step of loading HDI trimer on silica-alumina-based ceramic hollow microspheres includes: dropping HDI trimer into silica-alumina-based ceramic hollow microspheres, stirring evenly, and then treating with negative pressure to obtain silica-alumina-based ceramic hollow microspheres loaded with HDI trimer.

[0016] By adopting the above scheme, the loading process is simple, the HDI trimer is better loaded on the mesh structure on the surface of the silicon-aluminum-based ceramic hollow microspheres, and is better adsorbed by the physical cross-linking points and macromolecular chains of the silicon-aluminum-based ceramic hollow microspheres. The release rate of the HDI trimer and the reaction with polyaspartic acid ester is more appropriate, which can make the coating film smoother and denser after curing.

[0017] In a specific embodiment, the mass ratio of n-dodecyltriethoxysilane modified silica-alumina-based ceramic hollow microspheres and HDI trimer is 3:(4-4.1).

[0018] By adopting the above scheme, the HDI trimer can be better loaded on the n-dodecyltriethoxysilane modified silicon-aluminum-based ceramic hollow microspheres, and after being added to component A, the HDI trimer can be distributed more evenly. The silicon-aluminum-based ceramic hollow microspheres can achieve better thermal insulation effect in the coating, better loading effect on the HDI trimer and better improvement of the density of the coating of the present application.

[0019] In a specific embodiment, the vacuum degree is 0.08-0.09 MPa.

[0020] By adopting the above scheme, the HDI trimer is loaded on the silicon-aluminum-based ceramic hollow microspheres with good effect. The HDI trimer can also fill in some structural defects on the silicon-aluminum-based ceramic hollow microspheres, further prolonging the curing time, and will not affect the raw materials due to excessive pressure.

[0021] In a second aspect, the present application provides a method for preparing a solvent-free, moisture- and heat-resistant polyaspartic acid ester coating, comprising the following steps: stirring the raw material of component A evenly by mass to obtain a mixture, stirring the raw material of component B evenly by mass and then adding it to the mixture and mixing evenly to obtain a moisture- and heat-resistant polyaspartic acid ester coating.

[0022] In a specific embodiment, the raw material of component A is stirred uniformly by mass at a speed of 2000 rpm for 20 minutes, and the raw material of component B is stirred uniformly by mass at a speed of 700 rpm for 20 minutes.

[0023] By controlling the stirring speed and time of the coating components of the present application, the coating fineness is more uniform, and after curing, it is smoother, denser, and more resistant to moisture and heat.

[0024] In summary, this application has the following beneficial effects: This application uses polyaspartic acid ester, hydrophobic modified cellulose nanocrystals, and HDI trimer as the main components of the coating, which is solvent-free and environmentally friendly. By adding a certain amount of hydrophobic modified cellulose nanocrystals to component A to strengthen and protect the coating, especially cellulose nanocrystals modified by triethoxydiphenylsilane, polyaspartic acid ester infiltrates into the porous cellulose nanocrystals to extend the curing time, the long chains of silanes are intertwined with each other, the components in the coating are more tightly combined, the surface of the coating is smoother, and the hydrophobic groups associate with each other to form an elastic hydrophobic three-dimensional network structure to further protect the coating. Water vapor is not easy to invade under hot and humid conditions, and the stress of the coating is evenly dispersed, not easy to bubble under hot and humid conditions, and more resistant to hot and humid conditions.

[0025] The present application loads the HDI trimer in component B on hollow silicon-aluminum ceramic microspheres. The surface network structure of the hollow silicon-aluminum ceramic microspheres has physical crosslinking points that are easy to absorb resin and good macromolecular chain loading effect, which further improves the curing time of the coating. The obtained coating is smoother and more uniform, with fewer structural defects, and is not easy to be invaded by water vapor. The hollow structure is heat-insulated, making the internal structure of the coating more stable under hot and humid conditions. By modifying the hollow silicon-aluminum ceramic microspheres with n-dodecyl triethoxysilane, the dispersion effect, loading effect and winding effect are further improved, and the coating is denser. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments.

[0027] The polyaspartic acid ester is Bayer-NH1420, the HDI trimer is purchased from Mitsui Chemicals, Ltd. of Japan, the dispersant is KLK-2EHP from Malaysia, the defoaming agent is Sanshe-SS-605, the leveling agent is KMT-5519 leveling agent, the anti-settling agent is Tangyi-BYK-410, the light stabilizer is Youfeng-234, and the wetting agent is Evonik-Twin 4100.

[0028] Unless otherwise specified, the experimental reagents in the preparation examples and embodiments are conventional commercial brands or obtained through conventional preparation processes.

[0029] Preparation Example Preparation Example 1: Hydrophobic Modified Cellulose Nanocrystals 85 g of docosyltriethoxysilane was added to 900 ml of 95% ethanol aqueous solution, and ultrasonicated at room temperature for 10 minutes to obtain a hydrolyzate; 100 g of cellulose nanocrystals were added to 1000 ml of anhydrous ethanol to obtain a mixed solution; the hydrolyzate was dropped into the mixed solution, heated at 60°C, stirred and refluxed, reacted for 18 hours, cooled until crystals precipitated, filtered, and vacuum dried to obtain hydrophobically modified cellulose nanocrystals.

[0030] Preparation Example 2: Silicon-aluminum-based ceramic hollow microspheres loaded with HDI trimer 100 g of HDI trimer was dropped into 75 g of silicon-aluminum-based ceramic hollow microspheres, stirred evenly, and then subjected to negative pressure treatment with a vacuum degree of 0.09 MPa to obtain silicon-aluminum-based ceramic hollow microspheres loaded with HDI trimer.

[0031] Preparation Example 3: Silane-modified silica-alumina-based ceramic hollow microspheres 150 g of silica-alumina-based ceramic hollow microspheres and 100 g of n-dodecyltriethoxysilane were put into a 20% volume fraction ethanol aqueous solution, the pH value was adjusted to 2.5, nitrogen was introduced, heated at 90°C for 20 hours, washed with pure water three times, and dried in an oven at 55°C to obtain silane-modified silica-alumina-based ceramic hollow microspheres.

[0032] Preparation Example 4: Silane-modified silica-alumina-based ceramic hollow microspheres loaded with HDI trimer 150 g of silica-alumina-based ceramic hollow microspheres and 100 g of n-dodecyltriethoxysilane were put into a 20% volume fraction ethanol aqueous solution, the pH value was adjusted to 2.5, nitrogen was introduced, heated at 90°C for 20 hours, washed with pure water three times, and dried in an oven at 55°C to obtain silane-modified silica-alumina-based ceramic hollow microspheres.

[0033] 100 g of HDI trimer was dropped into 75 g of silane-modified silica-aluminum-based ceramic hollow microspheres, stirred evenly, and then subjected to negative pressure treatment with a vacuum degree of 0.09 MPa to obtain silane-modified silica-aluminum-based ceramic hollow microspheres loaded with HDI trimer.

[0034] Preparation Example 5: Hydrophobic Modified Cellulose Nanocrystals 85 g of n-dodecyltriethoxysilane was added to 900 ml of 95% ethanol aqueous solution, and ultrasonicated at room temperature for 10 minutes to obtain a hydrolyzate; 100 g of cellulose nanocrystals were added to 1000 ml of anhydrous ethanol to obtain a mixed solution; the hydrolyzate was dropped into the mixed solution, heated at 60°C, stirred and refluxed, reacted for 18 hours, cooled until crystals precipitated, filtered, and vacuum dried to obtain hydrophobically modified cellulose nanocrystals.

[0035] Preparation Example 6: Silane-modified silica-alumina-based ceramic hollow microspheres loaded with HDI trimer 150 g of silica-alumina-based ceramic hollow microspheres and 100 g of docosenyltriethoxysilane were put into a 20% volume fraction ethanol aqueous solution, the pH value was adjusted to 2.5, nitrogen was introduced, heated at 90°C for 20 hours, washed with pure water three times, and dried in an oven at 55°C to obtain silane-modified silica-alumina-based ceramic hollow microspheres.

[0036] 100 g of HDI trimer was dropped into 75 g of silane-modified silica-aluminum-based ceramic hollow microspheres, stirred evenly, and then subjected to negative pressure treatment with a vacuum degree of 0.09 MPa to obtain silane-modified silica-aluminum-based ceramic hollow microspheres loaded with HDI trimer.

[0037] Preparation Example 7: Silane-modified silica-alumina-based ceramic hollow microspheres loaded with HDI trimer 150 g of silica-alumina-based ceramic hollow microspheres and 100 g of n-dodecyltriethoxysilane were put into a 20% volume fraction ethanol aqueous solution, the pH value was adjusted to 2.5, nitrogen was introduced, heated at 90°C for 20 hours, washed with pure water three times, and dried in an oven at 55°C to obtain silane-modified silica-alumina-based ceramic hollow microspheres.

[0038] 110 g of HDI trimer was dropped into 75 g of silane-modified silica-aluminum-based ceramic hollow microspheres, stirred evenly, and then subjected to negative pressure treatment with a vacuum degree of 0.09 MPa to obtain silane-modified silica-aluminum-based ceramic hollow microspheres loaded with HDI trimer. Example

[0039] Example 1 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoamer, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 70g of hydrophobically modified cellulose nanocrystals obtained in Preparation Example 1, and Component B: 250g of HDI trimer.

[0040] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0041] Example 2 This example contains the following components: Component A: 350g of polyaspartic acid ester, 8g of dispersant, 2g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 70g of hydrophobically modified cellulose nanocrystals obtained in Preparation Example 1, and Component B: 200g of HDI trimer.

[0042] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0043] Example 3 This example contains the following components: Component A: 270g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 20g of hydrophobically modified cellulose nanocrystals obtained in Preparation Example 1, and Component B: 220g of HDI trimer.

[0044] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0045] Example 4 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 70g of hydrophobically modified cellulose nanocrystals obtained in Preparation Example 5, and Component B: 250g of HDI trimer.

[0046] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0047] Example 5 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 70g of hydrophobic modified cellulose nanocrystals prepared in Preparation Example 1, Component B: 437.5g of HDI trimer loaded on silica-alumina-based ceramic hollow microspheres prepared in Preparation Example 2.

[0048] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0049] Example 6 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 2-7g of hydrophobic modified cellulose nanocrystals prepared in Preparation Example 1, Component B: 437.5g of HDI trimer loaded on silane-modified silica-alumina-based ceramic hollow microspheres prepared in Preparation Example 4.

[0050] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0051] Example 7 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 2-7g of hydrophobic modified cellulose nanocrystals prepared in Preparation Example 1, Component B: 250g of HDI trimer, 187.5g of silane-modified silica-alumina-based ceramic hollow microspheres prepared in Preparation Example 3.

[0052] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0053] Example 8 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 2-7g of hydrophobic modified cellulose nanocrystals prepared in Preparation Example 1, Component B: 437.5g of HDI trimer loaded on silane-modified silica-alumina-based ceramic hollow microspheres prepared in Preparation Example 6.

[0054] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0055] Example 9 This example contains the following components: Component A: 200g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 2-7g of hydrophobic modified cellulose nanocrystals prepared in Preparation Example 1, Component B: 437.5g of HDI trimer loaded on silane-modified silica-alumina-based ceramic hollow microspheres prepared in Preparation Example 7.

[0056] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0057] Comparative Example Comparative Example 1 This comparative example contains the following components by mass: Component A: 400g of polyaspartic acid ester, 10g of dispersant, 1g of defoaming agent, 2g of leveling agent, 2g of anti-settling agent, 5g of light stabilizer, 1g of wetting agent, 70g of hydrophobic modified cellulose nanocrystals obtained in Preparation Example 1, and Component B: 250g of HDI trimer.

[0058] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0059] Comparative Example 2 This comparative example contains the following components by mass: Component A: 200g polyaspartic acid ester, 10g dispersant, 1g defoamer, 2g leveling agent, 2g anti-settling agent, 5g light stabilizer, 1g wetting agent, 70g cellulose nanocrystals, Component B: 250g HDI trimer.

[0060] The raw materials of component A are mixed by mass, stirred at a speed of 2000 rpm for 20 minutes to obtain a mixture, and the raw materials of component B are mixed by mass, stirred at a speed of 700 rpm for 20 minutes and then added to the mixture and stirred evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

[0061] Performance test test 1: The coatings prepared in each embodiment and comparative example were sprayed at 14MPa and 70℃, cured, and made into a coating film with a thickness of (1.5±0.2), and then placed in a constant temperature and humidity chamber for heat and humidity aging treatment, with a treatment time of 40 days, a treatment temperature of 85℃, and a treatment humidity of 85%. The coating shedding was tested and rated with reference to the standard ISO-2409-2007. The experimental results were graded according to the following judgment criteria: Grade 0: The cutting edge is completely smooth; no grid is shedding.

[0062] Level 1: A small amount of coating falls off at the intersection of the cuts. The cross-cut area affected cannot exceed 5%.

[0063] Grade 2: Coating is removed from cut edges and / or intersections. The affected cut area is greater than 5% but less than 15%.

[0064] Grade 3: The coating has partially or completely fallen off in large pieces along the cut edges and / or partially or completely fallen off in different parts of the grid. The affected cut area is greater than 15% but less than 35%.

[0065] Grade 4: Coating is falling off in large pieces along the cut edge and / or some cells are partially or completely falling off. The affected cut area is greater than 35% but less than 65%.

[0066] Grade 5: Any degree of shedding beyond Grade 4.

[0067] Test 2: The coatings prepared in each embodiment and comparative example were sprayed at 14 MPa and 70°C and cured to form a coating film with a thickness of (1.5±0.2). The surface drying time was then tested according to method B of GB / T 1728-1979, and the actual drying time was tested according to method C of GB / T 1728-1979.

[0068] Test 3: The coatings prepared in the embodiments and comparative examples were sprayed at 14 MPa and 70°C, cured, and formed into a coating film with a thickness of (1.5±0.2), and then the water permeability was tested at 0.4 MPa for two hours in accordance with the requirements of GT / B 23446-2009 "Spraying Polyurea Waterproof Coating".

[0069] The test results are summarized in Table 1.

[0070] Table 1 It can be seen from Examples 1-3 and Comparative Examples 1-2 and Table 1 that the coating prepared in the present application has good moisture and heat resistance by adding a certain amount of various additives in the polyaspartic acid ester coating and adding hydrophobic modified cellulose nanocrystals.

[0071] It can be seen from Example 1 and Example 4 and Table 1 that by limiting the long-chain silane of the hydrophobically modified cellulose nanocrystals to n-dodecyltriethoxysilane, the elastic waterproof network structure inside the obtained coating film is better in morphology, the curing time is appropriate, and the coating film is more uniform, dense and resistant to moisture and heat.

[0072] It can be seen from Example 1, Examples 5-9 and Table 1 that the present application prolongs the curing time of the coating to a certain extent by loading the HDI trimer on the silicon-aluminum-based ceramic hollow microspheres, and the obtained coating has good moisture and heat resistance.

[0073] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A solvent-free, heat-resistant polyaspartic acid ester coating, characterized in that: The invention comprises the following raw materials in parts by weight: component A: 20-35 parts of polyaspartic acid ester, 0.5-1 parts of dispersant, 0.1-0.2 parts of defoamer, 0.2-0.4 parts of leveling agent, 0.1-0.2 parts of anti-settling agent, 0.3-0.5 parts of light stabilizer, 0.1-0.3 parts of wetting agent, 2-7 parts of hydrophobic modified cellulose nanocrystals, and component B: 20-25 parts of HDI trimer.

2. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 1, characterized in that: The preparation steps of the hydrophobically modified cellulose nanocrystals include: adding long-chain silane to ethanol with a volume fraction of 90-95%, ultrasonicating for 7-12 minutes to obtain a hydrolyzate; adding cellulose nanocrystals to anhydrous ethanol to obtain a mixed solution; dripping the hydrolyzate into the mixed solution, heating at 55-60° C., stirring and refluxing, reacting for 18-19 hours, and then cooling, filtering, and vacuum drying to obtain the hydrophobically modified cellulose nanocrystals.

3. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 2, characterized in that: The long-chain silane is docosenyltriethoxysilane.

4. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 1, characterized in that: The HDI trimer of the B component is loaded on silica-alumina-based ceramic hollow microspheres.

5. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 4, characterized in that: The silicon-aluminum-based ceramic hollow microspheres are silicon-aluminum-based ceramic hollow microspheres modified by n-dodecyltriethoxysilane.

6. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 4, characterized in that: The step of loading the HDI trimer on the silicon-aluminum-based ceramic hollow microspheres comprises: dropping the HDI trimer into the silicon-aluminum-based ceramic hollow microspheres, stirring evenly, and then performing negative pressure treatment to obtain the silicon-aluminum-based ceramic hollow microspheres loaded with HDI trimer.

7. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 5, characterized in that: The mass ratio of the n-dodecyltriethoxysilane modified silicon-aluminum-based ceramic hollow microspheres and the HDI trimer is 3:(4-4.1).

8. The solvent-free heat-resistant polyaspartic acid ester coating according to claim 6, characterized in that: The vacuum degree of the negative pressure treatment is 0.08-0.09 MPa.

9. A method for preparing the solvent-free heat-resistant polyaspartic acid ester coating according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: uniformly stirring the raw material of component A according to mass to obtain a mixture, uniformly stirring the raw material of component B according to mass and then adding the raw material into the mixture and mixing evenly to obtain a moisture-heat resistant polyaspartic acid ester coating.

10. The method for preparing the solvent-free heat-resistant polyaspartic acid ester coating according to claim 9, characterized in that: The raw materials of component A are stirred uniformly by mass at a speed of 2000 rpm for 20 minutes, and the raw materials of component B are stirred uniformly by mass at a speed of 700 rpm for 20 minutes.

Citation Information

Patent Citations

  • Antistatic, heat-insulating and corrosion-resistance coating

    CN101812267A

  • High-strength polyaspartic acid polyurea waterproof coating and preparation method thereof

    CN111471380A

  • Polyaspartic acid ester polyurea coating and preparation method thereof

    CN112143352A

  • Solvent-free rain-erosion-resistant polyaspartic urea blade coating and preparation method thereof

    CN115637100A

  • Super-hydrophobic fabric as well as preparation method and application thereof

    CN116446182A

Cited By