High-yield-ratio Al-Mg alloy powder material for additive manufacturing as well as preparation method and application of high-yield-ratio Al-Mg alloy powder material
By using Al-Mg alloy powder materials with elements such as Mg, Mn, Zr, Ti, Ce, Si, etc. in 3D printed aluminum alloys, combined with laser additive manufacturing and aging heat treatment, the mechanical properties of aluminum alloy materials in the prior art are solved. and the problem of high cost, high yield strength and low cost aluminum alloy materials are achieved, suitable for load-bearing structural parts in aerospace and other fields.
Patent Information
- Application Number
- CN202411128752.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, the mechanical properties of 3D printed aluminum alloy materials are insufficient, the yield strength is difficult to reach 500MPa, and the cost is high, so it cannot replace forged aluminum alloys, and there is a lack of low-cost solutions that adapt to laser additive processes.
Al-Mg alloy powder material containing elements such as Mg, Mn, Zr, Ti, Ce, Si, etc. is prepared by vacuum air atomization method and laser additive manufacturing is carried out, combined with aging heat treatment to form an aluminum alloy member with a high yield strength ratio. , avoid the use of precious chemical elements.
The tensile strength of aluminum alloy materials is achieved ≥520MPa, yield strength ≥500MPa, and elongation ≥10%, reducing material costs, adapting to wide process windows, making it easy to industrial applications, and its performance exceeds that of forged high-strength aluminum alloys.
Smart Images

Figure CN118880132A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of laser additive manufacturing, and in particular to a high yield ratio Al-Mg alloy powder material for additive manufacturing and a preparation method and application thereof. Background Art
[0002] Powder bed laser additive manufacturing technology (3D printing for short) is mainly used for the near-net forming of high-precision, complex-shaped metal parts, providing tremendous impetus for the material-structure-function integrated design of key components in the fields of aerospace, weapons and equipment, biomedicine, and intelligent robots.
[0003] However, the engineering application of 3D printed aluminum alloy components is far less than that of titanium alloys. On the one hand, aluminum alloys have physical properties such as high laser reflectivity (91%), high thermal conductivity (237W / mK) and strong water absorption of powders, which are not compatible with the non-equilibrium solidification metallurgical process of laser additive manufacturing, resulting in a shortage of aluminum alloy powders available for 3D printing. Secondly, the relatively mature research on 3D printing Al-Si alloys, such as AlSi 10 Mg and AlSi7Mg have low strength of only 300-430MPa, which does not meet the design requirements of load-bearing structural parts (yield strength ≥ 500MPa), and yield strength is a key indicator of material service safety design, so it cannot replace the widely used forged aluminum alloys, such as 7000 series and 2000 series high-strength aluminum alloys. In addition, although according to literature reports and patent searches, 3D printing aluminum alloys with a yield strength of 500MPa can be found, such alloys usually contain more than 0.5wt% of rare earth Sc elements, resulting in an increase in the cost of powder raw materials, with a unit price of about 1000-1500 yuan / kg, even exceeding the price of titanium alloy powder (650 yuan / kg). Such high costs are difficult to meet market demand.
[0004] Based on the above problems, experts and scholars at home and abroad have done a lot of research on the micro-alloying design of Al-Zn-Mg-Cu, Al-Cu and Al-Mg-Si alloys, and basically solved the problems of metallurgical defect control and densification of 3D printed aluminum alloys, but the mechanical properties are always unsatisfactory, and the yield strength is difficult to reach 500MPa. For example, the document Selective laser melting additive manufacturing of 7xxx series Al-Zn-Mg-Cu alloy: cracking elimination by co-incorporation of Si and TiB2, Additive Manufacturing, 2020, 36: 101458 reported that by adding Si elements and nano-TiB2 particles, the formation of hot cracks in Al-Zn-Mg-Cu alloys can be suppressed to obtain highly dense 3D printed aluminum alloys, but the yield strength of the resulting material is only 460MPa. In addition, due to the introduction of nano-ceramic particles, the material has poor plasticity and an elongation of only 4.5%. Chinese patent CN113042748B discloses an Al-Cu-Mg alloy modified by Zr and Ti. The best room temperature tensile strength of the alloy is 487MPa, and the yield strength is only 366MPa. In addition, the laser cladding forming efficiency of the alloy is extremely low, with a scanning rate of only 200mm / s (the scanning rate of TC4 titanium alloy is 1200mm / s, and that of AlSi 10 Mg aluminum alloy scanning rate is 1300mm / s). Chinese patent CN117467875A discloses a Cu-modified Al-Mg-Si alloy with a multi-scale microstructure, and the room temperature yield strength of the alloy is 300-440MPa.
[0005] Up to now, my country still lacks low-cost (Sc-free) 3D printing aluminum alloy materials with excellent mechanical properties (yield strength ≥ 500MPa), good adaptability to laser additive manufacturing processes (wide process window), and industrial applicability. Summary of the invention
[0006] The present invention aims to at least partially overcome the above technical problems and / or other potential problems existing in the prior art: to provide a high yield ratio Al-Mg alloy powder material for additive manufacturing and a preparation method thereof. In order to obtain better application prospects and economic value and reduce costs, the 3D printing aluminum alloy prepared by the overall technical solution of the present invention does not contain precious chemical elements, and its mechanical properties reach or exceed the level of forged high-strength aluminum alloy, that is, tensile strength ≥520MPa, yield strength ≥500MPa, and elongation ≥10%.
[0007] The technical solution of the present invention is as follows: A high yield ratio Al-Mg alloy powder material for additive manufacturing, comprising the following chemical components, measured by mass percentage: Mg: 4.5-6.5wt%; Mn: 0.4-1.0wt%; Zr: 0.6-2.0wt%; Ti: 0.2-1.0wt%; Ce: 0.2-1.0wt%; Si: 0.2-0.3wt%; the rest is Al and unavoidable impurities; the sum of Zr, Ti and Ce is ≤2.4wt%, and the mass ratio of Zr to Ce is ≥2.
[0008] Preferably, the high yield ratio Al-Mg alloy powder material for additive manufacturing is a powder with a particle size of 15-63 μm, and the oxygen content of the powder is ≤500 ppm.
[0009] The present invention also provides a method for preparing the high yield ratio Al-Mg alloy powder material for additive manufacturing, the preparation method comprising the following steps: weighing raw materials according to a ratio, mixing the raw materials evenly and then melting them in a crucible, preparing Al-Mg alloy spherical powder by vacuum gas atomization, the atomizing gas being high-purity argon with a purity greater than 99.9%, and the powder being sieving through a grading device.
[0010] The present invention also provides an application of the high yield ratio Al-Mg alloy powder material for additive manufacturing, which is used to prepare aluminum alloy components. The preparation process includes the following steps:
[0011] 1) establishing a three-dimensional geometric model of the target part, slicing the model and designing the process, and using laser additive manufacturing technology to perform layer-by-layer cladding on the high yield ratio Al-Mg alloy powder material to obtain a deposited aluminum alloy component;
[0012] 2) Performing aging heat treatment on the deposited aluminum alloy component obtained in step 1 to obtain a high yield strength ratio 3D printed aluminum alloy component.
[0013] As an optimization, in step 1), a three-dimensional model of the required part is constructed using three-dimensional modeling software, and the model is converted into an STL file, which is then layered and discretized to set the processing parameters of the part to obtain the two-dimensional layered cross-sectional data and processing path of the part, and the file is imported into the laser additive manufacturing equipment to prepare for 3D printing.
[0014] As an optimization, in step 1), the high yield ratio Al-Mg alloy powder material is placed in a vacuum drying oven at 80-120° C. and dried for 1-2 hours before laser cladding to remove moisture adsorbed in the powder and improve powder fluidity.
[0015] As an optimization, in step 1), a laser additive manufacturing technology based on powder bed spreading is adopted, Al-Mg alloy powder is placed in a powder cavity, high-purity argon gas is introduced to ensure that the oxygen content in the equipment is less than 100 ppm, and a powder spreading scraper spreads a layer of powder on an aluminum substrate according to the layered slicing data. The substrate is preheated to 80-150°C in advance, and the laser selectively melts the powder according to a predetermined scanning path. The target part is obtained by layer-by-layer cladding deposition. The process parameters of laser additive manufacturing are: laser power 240-360W, scanning speed 400-1400mm / s, spot diameter <100μm, scanning spacing 90-120μm, powder layer thickness 30-90μm, and scanning strategy is partitioned island scanning.
[0016] As an optimization, in step 2), the aging heat treatment temperature is 320-360°C, the holding time is 2-4h, and the cooling method is air cooling or water cooling.
[0017] Preferably, the aging heat treatment temperature is 340° C. and the holding time is 2 h.
[0018] The beneficial effects of the present invention are as follows: on the one hand, the Zr, Ti and Ce elements added in the present invention are good nucleating agents, which refine the grains of the solidified structure and improve the grain boundary strengthening effect, thereby enhancing the mechanical properties of the alloy; the formed Al3Zr, Al3Ti and Al3(Ce, Zr) nano-dispersed phases can give the finished Al-Mg alloy a precipitation strengthening ability that the traditional grade Al-Mg alloy does not have, thereby significantly improving the material strength; the formation of the intermediate phase changes the microstructure and phase equilibrium of the Al-Mg alloy, effectively reducing the solidification temperature range of the Al-Mg alloy, making it more suitable for laser cladding additive manufacturing technology; and the prices of these three metal elements are much lower than Sc, which improves the material strength while meeting the low-cost requirements of industrial applications. On the other hand, in the high-rate additive manufacturing process, due to the fast movement speed of the laser and the work platform, the laser irradiation time is relatively short, so the formation and solidification time of the laser molten pool will be shortened accordingly. Mn and Si are beneficial elements for casting aluminum alloys, which can increase the fluidity of liquid metal. When the laser molten pool solidifies, the flowing liquid metal will be compensated in time, thereby avoiding the formation of defects such as pores and unfused, and improving the guarantee for high-rate additive manufacturing. In addition, Mn will form Al6Mn phase with Al to improve the corrosion resistance of the material; Si and Mg will form Mg2Si precipitation phase to improve the strength of the material. The strong ionic bond between Mg-Si will also reduce the burning loss of Mg element during laser cladding, thereby obtaining the expected material properties.
[0019] In summary:
[0020] 1) The high yield ratio Al-Mg alloy powder material for additive manufacturing described in the present invention does not contain expensive metal elements such as Sc. The 3D printing quality of Al-Mg alloy can be effectively improved by adding Zr, Ti and Ce elements, and the powder cost is greatly reduced, which has good economic value and industrial application prospects.
[0021] 2) The high yield ratio Al-Mg alloy powder material for additive manufacturing described in the present invention can adapt to a wider 3D printing process window, without the need to add special laser cladding processes such as laser remelting, dynamic laser pulse modulation, multi-laser beam technology, and molten pool shape control, which is convenient for mass production and can also adjust the printing efficiency according to the performance requirements of the actual workpiece. In comparison, the printing efficiency is higher and the process designability is strong.
[0022] 3) Compared with existing 3D printed aluminum alloys, the Al-Mg alloy prepared by the scheme of the present invention has a very high yield strength ratio (≥0.95) and outstanding mechanical properties. In a preferred embodiment, the tensile strength is 553 MPa, the yield strength is 516 MPa, and the elongation is 12.5%, reaching or even exceeding the level of forged 7000 series aluminum alloys and Sc modified aluminum alloys. The excellent strength-plasticity matching can meet the design requirements of load-bearing structural parts in the fields of aerospace, weapons and equipment.
[0023] 4) The Al-Mg alloy components prepared by the scheme of the present invention are heat-treatment-friendly and do not require solution heat treatment, thereby avoiding the risk of deformation and cracking of full-size 3D printed parts during quenching. Only a simple high-temperature aging treatment, i.e., 320-360°C insulation for 2-4 hours, can significantly improve the material strength, and achieve the dispersion strengthening effect of coexistence of multiple second phases of Al6Mn, Mg2Si, Al3Mg2, Al3Ti, Al3Zr and Al3(Ce,Zr) at the micron / nano scale. This high-temperature, short-time heat treatment is also beneficial to the release of residual thermal stress in 3D printed parts, further improving the uniformity of material organization and performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Example 1.
[0025] Figure 2 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Example 2.
[0026] Figure 3 This is the metal powder morphology after 3D printing Al-Mg alloy screening obtained in Example 3.
[0027] Figure 4 This is a linear scanning analysis of the chemical energy spectrum of the 3D printed Al-Mg alloy obtained in Example 3.
[0028] Figure 5 This is the micron / submicron equiaxed grain structure of the 3D printed Al-Mg alloy obtained in Example 3.
[0029] Figure 6 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Example 3.
[0030] Figure 7 This is the metallographic microstructure of the deposited cross section of the 3D printed Al-Mg alloy obtained in Comparative Example 1 after corrosion.
[0031] Figure 8 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Comparative Example 1.
[0032] Fig. 9 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Comparative Example 2.
[0033] Fig.10 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Comparative Example 3.
[0034] Fig.11 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Comparative Example 4.
[0035] Fig.12 This is the stress-strain curve of the 3D printed Al-Mg alloy obtained in Comparative Example 5.
[0036] Fig.13 This is the stress-strain curve of the 3D printed Al-Cu alloy obtained in Comparative Example 6. DETAILED DESCRIPTION
[0037] The present application is further described in detail below in conjunction with the accompanying drawings and examples, but the embodiments of the present invention are not limited to the scope of the examples. The examples are only used to illustrate the present invention, not to limit the scope of the present invention.
[0038] Example
[0039] Example 1
[0040] 1) weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, then using a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises magnesium Mg: 6.0wt%; manganese Mn: 0.7wt%; zirconium Zr: 0.7wt%; titanium Ti: 0.5wt%; cerium Ce: 0.2wt%; silicon Si: 0.2wt%; the rest is Al and unavoidable impurities.
[0041] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0042] 3) After the alloy powder was dried in a drying oven at 100°C for 2 h, it was placed in a selective laser melting equipment of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon gas was introduced to ensure that the oxygen content in the equipment was less than 100 ppm. The powder layer thickness was 30 μm, the laser power was 260 W, the scanning speed was 1000 mm / s, the spot diameter was 70 μm, the scanning spacing was 120 μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0043] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0044] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.85%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 527MPa, a yield strength of 502MPa, a yield strength ratio of 0.95, and an elongation of 12.9%. The corresponding stress-strain curve is as follows: Figure 1 shown.
[0045] Example 2
[0046] 1) Weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, then using a vacuum gas atomization device to prepare Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises magnesium Mg: 6.0wt%; manganese Mn: 0.7wt%; zirconium Zr: 1.0wt%; titanium Ti: 0.2wt%; cerium Ce: 0.2wt%; silicon Si: 0.2wt%; the rest is Al and unavoidable impurities.
[0047] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0048] 3) After drying the alloy powder in a drying oven at 100°C for 2 hours, the powder was placed in a selective laser melting device of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon was introduced to ensure that the oxygen content in the equipment was less than 100ppm. The powder layer thickness was 30μm, the laser power was 280W, the scanning speed was 1200mm / s, the spot diameter was 70μm, the scanning spacing was 120μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0049] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0050] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.88%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 532MPa, a yield strength of 510MPa, a yield strength ratio of 0.96, and an elongation of 12.1%. The corresponding stress-strain curve is as follows: Figure 2 shown.
[0051] Example 3
[0052] 1) Weigh the raw materials according to the ratio, mix them evenly and melt them in a crucible, then use a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieve it. After sieving, the powder size range is 15 to 63 μm, the oxygen content is ≤500 ppm, and the powder morphology is as follows: Figure 3 As shown, the chemical composition of the powder, by mass percentage, includes 6.0wt% magnesium Mg; 0.7wt% manganese Mn; 0.8wt% zirconium Zr; 0.5wt% titanium Ti; 0.4wt% cerium Ce; 0.2wt% silicon Si; and the rest is Al and unavoidable impurities.
[0053] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0054] 3) After drying the alloy powder in a drying oven at 100°C for 2 hours, the powder was placed in a selective laser melting device of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon was introduced to ensure that the oxygen content in the equipment was less than 100ppm. The powder layer thickness was 30μm, the laser power was 280W, the scanning speed was 1300mm / s, the spot diameter was 70μm, the scanning spacing was 120μm, and the scanning strategy was partitioned island scanning. After printing, the deposited aluminum alloy component was obtained, and the linear scanning analysis results of the material chemical energy spectrum are as follows: Figure 4 As shown in the figure, the actual average value of each element content is close to the preset value, and the fluctuation range of Mg element content at different locations is higher than that of other elements.
[0055] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0056] The final product was tested and the density of the aluminum alloy component prepared by this embodiment was 99.91%. Thanks to the addition of Zr, Ti and Ce ternary nucleating agents, the obtained aluminum alloy grains were fine and uniform, and its micron and submicron equiaxed fine grain structure was as follows: Figure 5 As shown in Figure 2, after being kept at 340℃ for 2h, the final material exhibits excellent mechanical properties, namely, room temperature tensile strength of 553MPa, yield strength of 516MPa, yield strength ratio of 0.93, and elongation of 12.5%. The corresponding stress-strain curve is shown in Figure 2. Figure 6 shown.
[0057] Comparative Example
[0058] Comparative Example 1
[0059] 1) Weigh the raw materials according to the ratio, mix the raw materials evenly and melt them in a crucible, then use vacuum gas atomization equipment to obtain Al-Mg alloy spherical powder and sieve it, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, includes magnesium Mg: 5.0wt%; manganese Mn: 0.7wt%; silicon Si: 0.2wt%; the rest is Al and unavoidable impurities, the composition refers to the existing commercial grade 5083Al alloy, without modification, and is directly used for subsequent laser additive manufacturing.
[0060] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0061] 3) After the alloy powder was dried in a drying oven at 100°C for 2 h, it was placed in a selective laser melting equipment of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon gas was introduced to ensure that the oxygen content in the equipment was less than 100 ppm. The powder layer thickness was 30 μm, the laser power was 280 W, the scanning speed was 1000 mm / s, the spot diameter was 70 μm, the scanning spacing was 120 μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0062] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0063] The final product was tested and the aluminum alloy component prepared by the comparative example could be formed, but the density was only 92.8%. Figure 7 As shown in Figure 2, there are obvious pores and cracks. After being kept at 340℃ for 2h, the room temperature tensile strength of the material is 303MPa, and the yield strength and elongation data cannot be obtained. The stress-strain curve is shown in Figure 2. Figure 8 shown.
[0064] Comparative Example 2
[0065] 1) weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, then using a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, includes magnesium Mg: 4.5wt%; manganese Mn: 0.7wt%; zirconium Zr: 0.7wt%; titanium Ti: 0.5wt%; the rest is Al and unavoidable impurities.
[0066] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0067] 3) After the alloy powder was dried in a drying oven at 100°C for 2 h, it was placed in a selective laser melting equipment of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon gas was introduced to ensure that the oxygen content in the equipment was less than 100 ppm. The powder layer thickness was 30 μm, the laser power was 280 W, the scanning speed was 1000 mm / s, the spot diameter was 70 μm, the scanning spacing was 120 μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0068] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0069] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.86%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 468MPa, a yield strength of 437MPa, a yield strength ratio of 0.93, and an elongation of 13.6%. The corresponding stress-strain curve is as follows: Fig. 9 shown.
[0070] Comparative Example 3
[0071] 1) Weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, then using a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises magnesium Mg: 5.0wt%; manganese Mn: 0.7wt%; zirconium Zr: 1.0wt%; titanium Ti: 1.5wt%; cerium Ce: 1.5wt%; silicon Si: 0.2wt%; the rest is Al and unavoidable impurities.
[0072] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0073] 3) After drying the alloy powder in a drying oven at 100°C for 2 hours, the powder was placed in a selective laser melting device of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon was introduced to ensure that the oxygen content in the equipment was less than 100ppm. The powder layer thickness was 30μm, the laser power was 280W, the scanning speed was 1000mm / s, the spot diameter was 70μm, the scanning spacing was 120μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0074] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0075] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.79%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 505MPa, a yield strength of 487MPa, a yield strength ratio of 0.96, and an elongation of 4.9%. The corresponding stress-strain curve is as follows: Fig.10 shown.
[0076] Comparative Example 4
[0077] 1) weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, using a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises magnesium Mg: 4.0wt%; manganese Mn: 0.6wt%; nickel Ni: 1.0wt%; the rest is Al and unavoidable impurities.
[0078] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0079] 3) After drying the alloy powder in a drying oven at 100°C for 2 hours, the powder was placed in a selective laser melting device of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon was introduced to ensure that the oxygen content in the equipment was less than 100ppm. The powder layer thickness was 30μm, the laser power was 280W, the scanning speed was 1000mm / s, the spot diameter was 70μm, the scanning spacing was 120μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0080] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0081] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.79%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 401MPa, a yield strength of 330MPa, a yield strength ratio of 0.82, and an elongation of 6.5%. The corresponding stress-strain curve is as follows: Fig.11 shown.
[0082] Comparative Example 5
[0083] 1) weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, using a vacuum gas atomization device to obtain Al-Mg alloy spherical powder and sieving, the powder size range after sieving is 15-63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises magnesium Mg: 4.0wt%; manganese Mn: 0.6wt%; titanium Ti: 0.2wt%; cerium Ce: 0.2wt%; nickel Ni: 1.0wt%; the rest is Al and unavoidable impurities.
[0084] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm and a solid support on the lower surface on the computer to facilitate the later processing of the tensile test bar; convert the three-dimensional model into an STL file and import it into the slicing software for slicing, design printing parameters and strategies, obtain the two-dimensional layered cross-section data and processing path of the part, and import the file into the selective laser melting equipment for subsequent printing processing.
[0085] 3) After drying the alloy powder in a drying oven at 100°C for 2 hours, the powder was placed in a selective laser melting device of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al substrate. The substrate preheating temperature before forming was 120°C, and pure argon was introduced to ensure that the oxygen content in the equipment was less than 100ppm. The powder layer thickness was 30μm, the laser power was 280W, the scanning speed was 1000mm / s, the spot diameter was 70μm, the scanning spacing was 120μm, and the scanning strategy was partitioned island scanning. After printing, a deposited aluminum alloy component was obtained.
[0086] 4) The deposited aluminum alloy components are subjected to aging heat treatment at a temperature of 340°C, a holding time of 2 hours, and an air cooling method to obtain high yield strength ratio 3D printed aluminum alloy components.
[0087] The final product was tested. The aluminum alloy component prepared by this embodiment had a density of 99.79%, good forming quality, no pores and cracks. After being kept at 340°C for 2h, the final material had a room temperature tensile strength of 469MPa, a yield strength of 371MPa, a yield strength ratio of 0.79, and an elongation of 12.6%. The corresponding stress-strain curve is as follows: Fig.12 shown.
[0088] Comparative Example 6
[0089] 1) Weighing raw materials according to the ratio, mixing the raw materials evenly and then melting them in a crucible, and preparing Al-Cu alloy spherical powder by vacuum gas atomization equipment, wherein the powder size range after screening is 15 to 63 μm, the oxygen content is ≤500 ppm, and the powder chemical composition, by mass percentage, comprises copper Cu: 5.0 wt%; magnesium Mg: 1.5 wt%; manganese Mn: 0.3 wt%; zirconium Zr: 1.0 wt%; titanium Ti: 0.5 wt%; and the rest is Al.
[0090] 2) Use Magics software to draw a cylindrical model with a diameter of 12 mm and a length of 80 mm on the computer for later processing of tensile test bars. After the model is converted into an STL file, it is imported into the slicing software for slicing, and the printing parameters and strategies are designed to obtain the two-dimensional layered cross-section data of the part, which is then imported into the selective laser melting equipment for subsequent printing processing.
[0091] 3) After the alloy powder was dried in a drying oven at 110°C for 2 h, it was placed in a selective laser melting equipment of model EOS M290 for layer-by-layer printing. The substrate material was 6061Al. The substrate preheating temperature before forming was 120°C, and high-purity argon gas was introduced to ensure that the oxygen content in the equipment was less than 100 ppm. The powder layer thickness was 30 μm, the laser power was 240 W, the scanning speed was 200 mm / s, the spot diameter was 70 μm, the scanning spacing was 120 μm, and the scanning strategy was partitioned island scanning.
[0092] 4) The aluminum alloy component prepared by this embodiment has a density of 99.3% and no obvious pores and cracks. After being kept at 525°C for 2 hours and then water-cooled, the final material has a room temperature tensile strength of 457MPa, a yield strength of 366MPa, a yield strength ratio of 0.80, and an elongation of 11.4%. The corresponding stress-strain curve is as follows: Fig.13 shown.
[0093] The chemical compositions of the above embodiments and comparative examples are shown in Table 1, and the mechanical properties test results are shown in Table 2.
[0094] Table 1 Chemical composition of the embodiments and comparative examples (in mass percentage)
[0095]
[0096]
[0097] Table 2 Mechanical properties of the embodiments and comparative examples
[0098] Tensile strength(MPa) Yield strength(MPa) Elongation(%) Yield-to-strength ratio Example 1 527 502 12.9 0.95 Example 2 532 510 12.1 0.96 Example 3 553 516 12.5 0.93 Comparative Example 1 303 / / / Comparative Example 2 468 437 13.6 0.93 Comparative Example 3 505 487 4.9 0.96 Comparative Example 4 401 330 6.5 0.82 Comparative Example 5 469 371 12.6 0.79 Comparative Example 6 457 366 11.4 0.80
[0099] It can be seen from the examples and comparative examples that the advantages of the technical solution of the present invention are obvious. Compared with comparative example 1, examples 1-3 add appropriate amounts of Zr, Ti and Ce elements, which effectively improve the process adaptability of AlMg alloy laser forming and eliminate metallurgical defects such as holes and cracks. Comparative example 2 is modified only by adding Zr and Ti, and the mechanical properties are limited, and the yield strength of the final product is less than 500MPa. The total amount of Zr, Ti and Ce elements added in comparative example 3 is too high, and the excess alloying elements will not continue to improve the strength of the material, and even deteriorate the plasticity of the material, resulting in a decrease in elongation. The modification effect of the Ni element in comparative examples 4 and 5 is far inferior to that of the Zr element. It can be seen from the stress-strain curve that the obtained material has an obvious work hardening effect, and the mechanical properties are shown as a low yield strength ratio. Comparative example 6 is an AlCu alloy modified by Zr and Ti. This series of alloys requires solid solution heat treatment, which is easy to cause parts to deform, and has a low yield strength, with a yield strength ratio of only 0.80, and the mechanical properties are far inferior to the materials obtained in examples 1-3.
[0100] The above are only examples of the features of the present invention and do not constitute any limitation on the protection scope of the present invention. Any technical solution formed by equivalent exchange or equivalent replacement falls within the protection scope of the present invention.
Claims
1. A high yield ratio Al-Mg alloy powder material for additive manufacturing, It is characterized in that The invention comprises the following chemical components in terms of mass percentage: Mg: 4.5-6.5wt%; Mn: 0.4-1.0wt%; Zr: 0.6-2.0wt%; Ti: 0.2-1.0wt%; Ce: 0.2-1.0wt%; Si: 0.2-0.3wt%; the rest are Al and unavoidable impurities; the sum of Zr, Ti and Ce is ≤2.4wt%, and the mass ratio of Zr to Ce is ≥2.
2. The high yield ratio Al-Mg alloy powder material for additive manufacturing according to claim 1, It is characterized in that The powder particle size is normally distributed in the range of 15-63 μm, and the powder oxygen content is ≤500 ppm.
3. A method for preparing the high yield ratio Al-Mg alloy powder material for additive manufacturing as claimed in any one of claims 1 or 2, It is characterized in that The preparation method comprises the following steps: weighing raw materials according to a ratio, mixing the raw materials uniformly and then melting them in a crucible, preparing Al-Mg alloy spherical powder by vacuum gas atomization, the atomizing gas is high-purity argon gas with a purity greater than 99.9%, and the powder is sieved by a grading device.
4. An application of the high yield ratio Al-Mg alloy powder material for additive manufacturing as claimed in any one of claims 1 or 2, It is characterized in that For preparing aluminum alloy components, the preparation process includes the following steps: 1) establishing a three-dimensional geometric model of the target part, slicing the model and designing the process, and using laser additive manufacturing technology to perform layer-by-layer cladding on the high yield ratio Al-Mg alloy powder material to obtain a deposited aluminum alloy component; 2) Performing aging heat treatment on the deposited aluminum alloy component obtained in step 1 to obtain a high yield strength ratio 3D printed aluminum alloy component.
5. Application of the high yield ratio Al-Mg alloy powder material for additive manufacturing according to claim 4, It is characterized in that In step 1), a 3D model of the required part is constructed using 3D modeling software, the model is converted into an STL file, and then layered discretization is performed to set the processing parameters of the part to obtain the 2D layered cross-sectional data and processing path of the part, and the file is imported into the laser additive manufacturing equipment to prepare for 3D printing.
6. Application of the high yield ratio Al-Mg alloy powder material for additive manufacturing according to claim 4, It is characterized in that In step 1), the high yield ratio Al-Mg alloy powder is placed in a vacuum drying oven at 80-120° C. and dried for 1-2 hours before laser cladding.
7. Application of the high yield ratio Al-Mg alloy powder material for additive manufacturing according to claim 4, It is characterized in that In step 1), a laser additive manufacturing technology based on powder bed spreading is adopted, Al-Mg alloy powder is placed in a powder cavity, and high-purity argon gas is introduced to ensure that the oxygen content in the equipment is less than 100ppm; according to the layered slicing data, a powder spreading scraper spreads a layer of powder on an aluminum substrate, the substrate is preheated to 80-150°C in advance, and the laser selectively melts the powder according to a predetermined scanning path, and the target part is obtained by layer-by-layer cladding deposition. The process parameters of laser additive manufacturing are: laser power 240-360W, scanning speed 400-1400mm / s, spot diameter <100μm, scanning spacing 90-120μm, powder layer thickness 30-90μm, and scanning strategy is partitioned island scanning.
8. Application of the high yield ratio Al-Mg alloy powder material for additive manufacturing according to claim 4, It is characterized in that In step 2), the aging heat treatment temperature is 320-360° C., the holding time is 2-4 hours, and the cooling method is air cooling or water cooling.
Citation Information
Cited By
Heat-resistant aluminum alloy material as well as preparation method and application thereof
CN120796786A
A heat-resistant aluminum alloy material and a preparation method and application thereof
CN120796786B
Additive manufacturing Al-Cu-Sc alloy and high-toughness preparation method thereof
CN121472663A