Laser deposition welding method for producing a coating layer on a component
By using spiral or spiral rail lines and winding overlap technology in laser deposition welding, the problem of increasing the surface wave degree of the coating layer in traditional methods is solved, and high-quality and efficient coating layer manufacturing is achieved, reducing the Depth grinding of component surfaces requires.
Patent Information
- Application Number
- CN202380021713.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2023-02-14
- Publication Date
- 2024-11-01
Smart Images

Figure CN118891128A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a laser deposition welding method for producing a coating on the surface of a component, a device for carrying out the laser deposition welding method and a component having at least one surface coated with a coating, wherein the coating is produced by means of the laser deposition welding method. Background Art
[0002] Conventional laser deposition welding methods are known from the prior art. In this process, the surface of the component is melted by means of a laser beam and the melt pool formed thereby is supplied with powdered additive material. The powder is then also melted in the melt pool, so that after solidification of the molten powder material and the surface, a material layer is formed which is bonded in a material-locking manner, in particular metallurgically fused.
[0003] Depending on the application, this process can be carried out at different points on the surface or also on larger continuous areas of the workpiece surface, so that three-dimensional shapes can be applied with the help of laser deposition welding. In addition, multiple material layers composed of different materials can be constructed on the surface one above the other. If a metallic material is applied, the deposition method is also called "Laser Metal Deposition" (LMD for short). Typical application areas of laser deposition welding are repair, coating and joining technology.
[0004] So-called extremely high-speed laser deposition welding (EHLA for short) is already known from DE 10 2011 100 456 B4. According to this method, the achievable processing speed is significantly increased compared to conventional laser deposition welding by supplying at least one additive material in an at least partially molten state to the process zone on the surface to be processed. For this purpose, the additive material, which is initially present in powder form, is melted by means of a laser beam at a distance greater than zero, in particular melted into a molten pool, and then supplied to the molten pool in an especially completely liquid form. The melting of the additive material, in particular the powder, at the mentioned distance from the molten pool and the heating of the molten pool can be carried out by the same laser beam. Therefore, the laser beam incident on the molten pool also melts the additive material at the mentioned distance from the molten pool. This can be achieved by moving the molten pool and the focus of the laser beam parallel to each other relative to the surface at a speed of at least 20 m / min. In addition, when using a powdered additive material, the powder density can be set in particular such that the laser power of the laser beam in the molten pool is less than 60% of the laser power before the laser beam comes into contact with the powder. Thus, the processing speed of the laser deposition welding method can be significantly increased by means of the EHLA method.
[0005] The coating structure (which can also be formed on the opposite surface of the component) can have a layer thickness between 50 μm and 500 μm, preferably between 100 μm and 200 μm, which can be generated in particular by the track width of the track that passes through the molten pool several times. In industrial development, in order to increase the productivity (welding area per unit time), increasingly larger laser powers are used, for example laser powers in the focus of up to 24 kW. By increasing the laser power, the coating spot size (laser focus diameter and powder focus diameter) must or is increased. More area can be processed on the processing trajectory per unit time. Surprisingly, experimental results show that with an increase in the irradiation spot diameter or the laser power, the surface waviness of the coating welded by means of high-speed LMD also increases. Therefore, a large margin for the layer thickness must be set so that the coating has an ideal surface finish (especially roughness) after subsequent grinding. The coating must be ground below the resulting valleys of the wavy coating. Summary of the invention
[0006] The object of the present invention is to reduce the above-mentioned disadvantages of the laser deposition welding method and in particular to improve the quality of the produced component by reducing the surface waviness of the produced coating.
[0007] This object is achieved by a laser deposition welding method according to claim 1. A laser deposition welding method is proposed for producing a coating on a surface of a component, in which at least one coating track with a predetermined track width is produced on the surface by applying an additive material (in particular in powder form) along a helical or spiral processing path, wherein the additive material and the component are heated along the processing path by means of a laser beam so that at least one coating track is produced when the additive material strikes the surface, wherein at least two turns (in particular at least three turns) of at least one coating track at least partially overlap or are produced at least partially overlapping along the track width. In particular, the laser focus diameter of the laser beam can be greater than 1 mm, in particular 1.4 mm to 12 mm.
[0008] By laser deposition welding, two, three or more turns of at least one coating track (the coating track forms a coating layer or a part of a coating layer by solidification) are produced in particular side by side along the track width, so that the turns are adjacent to each other with partial overlap, which has been proven to effectively reduce the surface ripples of the coating layer produced in this way. Here, the turns are produced in particular side by side and partially overlapping each other. Advantageously, a particularly high laser power can be achieved, so that the productivity of the laser deposition welding method can be increased without reducing the quality of the manufactured components or requiring depth compensation grinding of the coating layer. It is particularly advantageous here that on the entire at least one coating track, on average, at least four or more turns that partially overlap each other are produced side by side along the track width to produce the coating layer on the component. In addition, it is particularly possible to produce the entire coating layer with only a single coating track, which has a corresponding number of turns along a spiral or spiral processing trajectory. In this regard, the coating track produced along the processing trajectory is particularly produced continuously and without interruption. However, it is also possible to interrupt the processing and use two or more coating tracks, wherein the coating tracks can be placed adjacent to each other.
[0009] The term "windings that at least partially overlap each other along the track width" refers here to how many windings of at least one coating track are coated on each track width. In particular, the number of windings that are visible on each track width of the at least one coating track in a top view of the at least one coating track or the coating layer produced is calculated. Therefore, the windings that partially overlap each other do not need to extend completely within a track width, because in this way the windings will completely overlap each other, rather than just partially overlapping. Here, the partial overlap of the windings refers to the overlapping width of the windings. In principle, the number of windings along the track width does not have to be an integer, and may also include parts of an integer. For example, 4.1 or 4.6 windings may partially overlap each other along the track width and be arranged side by side.
[0010] According to the invention, it is proposed that the windings produced side by side overlap each other at least partially, but it can also be proposed, as mentioned at the beginning, that the windings of the at least one coating track are produced overlapping each other by sweeping the track width several times in order to produce a coating layer of a certain thickness, for example in the range of 50 μm to 300 μm, preferably with a thickness of 100 μm. In contrast to the side-by-side production of windings that at least partially overlap each other, the windings of the at least one coating track are not produced side by side here. Instead, the track width or winding that has already been produced or traveled through is usually swept again only after the entire processing trajectory has been passed through.
[0011] In particular, it can be provided that, on the turns in the beginning and / or end region of the processing path, further turns are produced on the path width thereof. In other words, as described above, a path width can be swept several times, particularly in the beginning and / or end region of the processing path. This has the advantage of producing a constant coating thickness, for example in the case of brake disks as components on the outer and / or inner circumference of the friction surface to be coated.
[0012] It can be provided that at least four at least partially overlapping windings are produced side by side along the track width. Surprisingly, only particularly small surface waviness of the coating is produced by the four partially overlapping windings, in which respect the coating does not have to be reprocessed or can be reprocessed only by slight regrinding.
[0013] It can also be provided that the windings which partially overlap each other overlap each other by at least 20%, in particular by at least 40%, of the track width. In particular, the degree of overlap, which is described here by way of example as a percentage of the track width, can be substantially the same in the case of the windings. It has been found that this degree of overlap also produces particularly low surface waviness of the coating.
[0014] Furthermore, it can be provided that during the production of the processing layer, the number of windings which at least partially overlap one another along the track width can be varied. In particular, the number of windings can be varied within 50% of the average number of windings which partially overlap one another along the track width and / or the degree of overlap can be varied within 50% of the average degree of overlap over all windings. This has the advantage that the coating thickness can be adjusted during the laser deposition welding process. Furthermore, during the control operation of the laser deposition welding process, the coating thickness can be guided around a target value and, in the case of so-called umbrella-shaped disks, mutually opposite surface-parallel surfaces of the component can be produced by the coating thickness extending in a wedge-shaped manner.
[0015] Furthermore, it can be provided that a height profile of a surface coated with at least one coating track is generated by means of a measuring device. For example, the measuring device can be provided for optical cross-sections. For example, the measuring device can also be an optical coherence tomography or a thermography measuring device. The advantage of such a measuring device is that undesired waviness of the coating can be monitored by means of the height profile generated. Furthermore, the height profile or a parameter indicating the waviness of the coating derived from the height profile can be compared with a predetermined limit value. When the predetermined limit value is exceeded, the manufacturing process can be stopped automatically or a regulatory intervention can be made in the laser deposition welding process to reduce the waviness.
[0016] It can be provided that the point of incidence of the laser beam on the surface can be moved along the surface at a relative speed of at least 20 m / min. The relative speed is the speed at which the surface to be coated moves relative to the point of incidence of the laser beam on the surface. The laser beam is incident on the surface in such a way that a processing zone is generated on the surface, in particular a molten pool is at least partially generated on the surface. Thus, it can also be said that the point of incidence and thus the processing zone are displaced along the surface at a speed of at least 20 m / min. The main advantage of such a high relative speed is that a very high productivity can be achieved. Such laser deposition welding can also be referred to as high-speed laser deposition welding.
[0017] Furthermore, it can be provided that the component is rotationally symmetrically constructed, in particular as a disk, and is rotated about an axis of rotation, in particular during the production of the coating layer, so that the processing trajectory follows a spiral or helical shape. For example, the component can be a brake disk, a sliding disk, a friction disk or a similar component, which can be used in various applications, for example in motor vehicles. The surface to be coated or the surfaces to be coated opposite each other can be annular surfaces in this case. Accordingly, the rotation of the disk about its axis of rotation allows the disk to be coated circumferentially. For this purpose, the disk can be fastened to the shaft of a corresponding drive device (for example an electric motor), which rotates the disk. In addition, the point of incidence of the laser beam can naturally also be moved, in particular linearly. In particular, the laser beam can be moved in a plane above the disk. This can be achieved, for example, by a linear drive on a processing head, which emits the laser beam. The supply orientation of at least one additive material can also be moved respectively together with the point of incidence of the laser beam.
[0018] Furthermore, it can be provided that at least one additive material is present as a powder before the melting by means of the laser beam. The additive material can be metallic. In addition to the metallic additive material, other materials can also be present, which are to be added to the coating. Furthermore, different metals can also be processed. Alternatively, it is conceivable that the additive material can also be present as a wire, a strip or a sheet. However, it is particularly advantageous to supply the powdered additive material to the laser beam for melting so that it is supplied to the processing zone in essentially completely molten form.
[0019] Furthermore, it can be provided that at least one additive material is supplied to the corresponding laser beam by at least three injectors on each surface of the component. Preferably, there are in particular 3 to 21 injectors, in particular 7 to 14 injectors, per surface or side of the component. This allows a very symmetrical focus of the additive material, in particular a powder focus, to be produced on the surface, thereby improving the quality of the produced coating.
[0020] Furthermore, it can be provided that the average powder efficiency of all injectors for using powdered additive material is at least 85% in total. The powder efficiency indicates how much of the supplied powder is melted. Powder losses can thus be reduced. This is achieved in particular by using injectors that are arranged at an angle of 90° to the direction of gravity.
[0021] Furthermore, it can be provided that the injectors can be supplied with powder via two or more supply lines from corresponding powder conveyors, which powder can be directed to two or more injector groups via a distributor component. Thus, the required powder mass flow can be distributed into parallel powder supply branches. Thus, a particularly uniform powder mass flow is achieved and thus a particularly uniform coating layer is produced.
[0022] The injectors can advantageously be designed as tubes. In particular, they can be designed as hard metal tubes in order to have a high resistance to the additive material on the one hand and to the high temperatures resulting from the process on the other hand. The advantage of the tubes is also that a particularly good flow of a possible conveying gas through the tubes is provided in order to supply the additive material from a corresponding conveyor or reservoir to the laser beam at a distance from the surface.
[0023] Furthermore, it can be provided that the outlet angle of the injector relative to the perpendicular to the corresponding surface of the component is less than 60°, in particular less than 50°, and in particular less than 40°. It has been shown that the surface waviness of a coating welded in this way is particularly low.
[0024] Furthermore, it can be provided that at least one additive is supplied to the laser beam by means of a conveying gas, wherein the conveying gas has a relative atomic mass of at least 4, in particular at least 14, and / or has a relative atomic mass of 1.5 Å per mm 2 A specific volume flow of at least 3.2 Nl / min over the cross-sectional area. It has been shown that a conveying gas having the above parameters provides a sufficiently strong impulse and thus a high feed material velocity, in particular a powder velocity, so that the feed material can be guided onto the laser beam without being significantly influenced by external factors, such as the gravity acting on the feed material, and thus with optimal effect.
[0025] Furthermore, it can be provided that the coating of the component is produced in the direction from the relatively inner side of the surface to the relatively outer side of the surface. In the case of a disk as a component, the coating or the movement of the laser beam spot is thus carried out from the radial inner side or the inner diameter to the radial outer side or the outer diameter. In this way, thermal expansion can be utilized to generate tensile stresses in the component, in particular the disk. During cooling, the welded coating develops compressive stresses. This is advantageous because compressive stresses can counteract crack progression in the welded coating.
[0026] Furthermore, it can be provided that the laser beam axis of the laser beam is tilted relative to the surface at an angle of incidence greater than a range of 0° to 35°, in particular a range of 5° to 30°. For this purpose, the main axis of the processing head from which the laser beam is emitted can be tilted accordingly relative to the surface. In this way, laser light reflected from the component at the angle of incidence does not strike the processing head, but is deflected away from it.
[0027] Furthermore, it is possible to generate the intensity distribution of the laser beam in at least approximately the form of a so-called flat top. It has been shown that such a distribution produces less roughness on the coating layer than a Gaussian laser power distribution. In particular, the intensity distribution can be approximately in the form of a flat top with an intensity range that decreases in the center (I_max (maximum intensity) ≥ I_core (core intensity) ≥ 0). This opens up a particularly large process window for laser deposition welding processes.
[0028] The object mentioned at the outset is also achieved by a component according to claim 14 , which has a surface provided with a coating, wherein the coating is produced by means of the laser deposition welding method according to the invention.
[0029] Tracks which partially overlap one another over the track width can be seen under a microscope in a cross section of the component, so that components produced by means of a laser deposition welding method can be clearly distinguished from components whose coatings were produced by means of a different method.
[0030] Features described herein in relation to the laser deposition welding method are equally applicable to the component, and vice versa.
[0031] The object mentioned at the outset is also achieved by a device according to claim 15. The device is configured to carry out the laser deposition welding method according to the invention, wherein the device has at least one laser for generating a laser beam, wherein the device has at least one additive feeder for feeding at least one additive to the laser beam at a distance from the component surface.
[0032] Features described herein in relation to the laser deposition welding method and component are equally applicable to the apparatus, and vice versa, respectively.
[0033] In particular, the device has a regulating and / or control device which is provided for regulating and / or controlling the laser deposition welding process such that at least two turns or at least three turns of at least one coating track overlap along the track width. For this purpose, a regulating and / or control program with corresponding instructions can be provided in the regulating and / or control device.
[0034] At least one laser can have a laser power of preferably more than 4 kW, in particular more than 12 kW and up to 24 kW. For example, it can be a laser with a wavelength of about 1 μm (fiber laser, disk laser), about 0.8 μm (diode laser) or 0.5 μm (green light converter). Laser cables with two-in-one optical fibers can be used, wherein core diameters of 600 μm to 1000 μm, or diameter ratios of 200 μm / 700 μm and 300 μm / 1000 μm can be implemented. An adjustment device (wedge switch) can also be used to set the core-cladding ratio of the two-in-one optical fiber. The processing head of the laser can have a focal length of about 1.4 mm to about 8 mm for imaging the fiber end of the two-in-one optical fiber in the region of the powder focus or on the surface.
[0035] At least one additional material conveyor can be designed as a powder conveyor and have a powder nozzle for forming a powder focus. As described above, the powder nozzle can be implemented by means of an injector, in particular using a plurality of injectors as a multi-nozzle. Inert gases such as argon or helium or mixtures thereof can be used as conveying gases. It is also possible to supply process shielding gases to the process.
[0036] Furthermore, other devices, such as the above-mentioned measuring devices, component receiving parts, etc., can naturally be provided in the device.
[0037] Further details and advantageous embodiments of the invention can be found in the following description, in which the invention is described and explained in more detail with the aid of its exemplary embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] It shows:
[0039] Figure 1 A schematic view of the structure of an apparatus for a laser deposition welding method;
[0040] Figure 2 A top view of a component according to an embodiment of the present invention;
[0041] Figure 3 A top view of a component when coated by a laser deposition welding method according to an embodiment of the present invention;
[0042] Figure 4a , 4b is a schematic view of a laser deposition welding method according to an embodiment of the present invention;
[0043] Figure 5 , 6 a cross-sectional view of a portion of a component when coated by different laser deposition welding methods;
[0044] Figure 7 , 8 by Figure 5 and Figure 6A top view of a portion of a component when coated by different laser deposition welding methods; and
[0045] Figure 9-13 Cross-sections of components coated according to different laser deposition welding methods. DETAILED DESCRIPTION
[0046] In the following description and in the drawings, identical or mutually corresponding features are provided with the same reference numerals.
[0047] Figure 1 The overall diagram shows a device 10 for laser deposition welding. The device 10 includes a laser 12 for generating a laser beam 1. The generated laser beam 1 is supplied to a light outlet 16 via an optical waveguide cable 14. The laser beam 1 generated thereby is aligned in parallel in a collimating lens 18. The laser beam 1 then passes through a movable processing head 20 (in addition, the light outlet 16 and the collimating lens 18 can also be installed in the processing head 20 instead). A focusing lens (not shown) is arranged in the processing head 20 for focusing the laser beam 1. After passing through the focusing lens, the laser beam 1 passes through a cylindrical section 22 and a funnel-shaped section 24 of a processing head 26, which also serve as powder nozzles for powdery additive material 2.
[0048] The entire assembly consisting of the light outlet 16, the collimating lens 18 and the processing head 22 can be arranged linearly movably above the component 70 to be coated by means of the feed unit 30. More precisely, the feed unit 30 can be arranged in a plane spanned by the X-coordinate and the Y-coordinate on the component 70 (see Figure 2 ). For example, the feed unit 30 currently comprises a linear drive 34 and an electric motor 32 driving the linear drive 34. In addition, the device 10 comprises a rotation unit 90, which currently has an electric motor 92 with a shaft 94 coupled thereto for rotating the component 70 mounted thereon. The component 70 is here, for example, rotationally symmetrically designed, in particular as a brake disk, and rotates about its axis of rotation 72, which coincides with the axis 94, when the component 70 is coated with the coating layer 80 in the illustrated direction of rotation R, which will be described in detail later.
[0049] The device 10 also includes an additive material conveyor 40 for conveying a powdered additive material 2. In the additive material conveyor 40, the powder is mixed with a gas, in particular an inert gas such as nitrogen or argon, to produce a powder gas flow 4 for conveying the powder. In the distributor member 42, the powder gas flow 4 is distributed to a plurality of supply lines 44 (three in the present case), in particular supply hoses, and then flows into the cylindrical section 22 of the processing head 20. The section 24 of the processing head 20 has a double wall, wherein the powder gas flow is guided through the annular gap thus created, so that the powder gas flow 4 flows between the two walls. Therefore, the laser beam 1 and the powder gas flow 4 extend coaxially to each other through the sections 22 and 24. Here, in the funnel-shaped section 24, the annular gap between the two walls is narrowed, and the powder gas flow 4 leaves through the nozzle-shaped outlet of the funnel-shaped section 24 thus formed.
[0050] The device 10 also includes a sensor measuring device 50. For example, the measuring device 50 can be configured to perform a light section method to generate a height profile of the surface 74. Here, for example, a light section scan can be performed at 4 kHz. In particular, a height profile can be generated along the schematically shown projected light 52.
[0051] Finally, the device 10 comprises a regulating device 60. The regulating device serves, on the one hand, to control the laser 12 and the additive material conveyor 40. The regulating device serves, on the other hand, to actuate a control unit 62, which also belongs to the device 10 and is designed to actuate the electric motor 32 and the further electric motor 92. Furthermore, the regulating device 60 is provided for evaluating the measurement signals detected by the measuring device 50. For example, the regulating device 60 can measure the height profile of the coating 80 and compare it with a predefined limit value for the maximum waviness of the coating 80. If the limit value is exceeded, the regulating device 60 can intervene accordingly by means of regulating measures.
[0052] Figure 2 A component 70 in the form of a brake disk for a motor vehicle is shown, wherein a surface 74 has a coating 80 which is produced by the method described below. Such a coating 80 can also be produced on the opposite surface 74 or side of the component 70 .
[0053] In summary, the apparatus 10 is configured to implement the method described below:
[0054] The presently annular surface 74 of the component 70 is coated by means of the device 10 by means of extremely high speed laser deposition welding (EHLA). To this end, the component 70 is first rotated by the shaft 94 being driven by the further electric motor 92 .
[0055] Furthermore, a laser beam 1 is generated and projected onto a surface 74, wherein the laser beam 1 impinges on the surface 74 at an incident point. A processing zone 6 is thereby generated on the surface 74. Furthermore, a powder gas flow 4 is generated. After leaving the cylindrical section 24, the powdered additive material 2 of the powder gas flow 4 hits the optical path of the laser beam 1 during its flight phase. As a result, the additive material 2 in the form of powder particles is at least partially or completely melted before reaching the processing zone 6 on the component 70. Therefore, the additive material 2 is preferably supplied to the processing zone 6 in a completely molten form. The additive material 2 melted by the heating of the laser beam 1 is then applied to the surface 74 of the component 70. Here, the component 70 rotates rapidly about the rotation axis 72, and the incident point of the laser beam 1 is along a predetermined processing trajectory 88 (see Figure 3 ) is displaced on the surface 74 at a speed of at least 20 m / min, which can also be described as high-speed laser deposition welding. Thus, the processing zone 6 generated by means of the laser beam 1 is displaced along the surface 74 at a speed of at least 20 m / min. Thus, at least one coating track 86 is generated along the processing track 88 by means of the molten additional material 2, which will be referred to below. Figure 3 Provide detailed explanation.
[0056] The coating layer 80 is gradually produced by the laser deposition welding process. Figure 3 Purely by way of example, the laser beam 1 is here moved in sections from the radial outside to the radial inside relative to the rotation axis 72 by means of a linear drive 34, so that the point of incidence of the laser beam 1 moves along the surface 74 in a spiral processing path 88. Thus, at least one coating path 86 with a plurality of turns 8 is generated along the processing path 88, which extend around one another or around the center point of the component 70. The coating path 86 or turns 8 are preferably generated continuously here, i.e. without processing stops, and moreover, in particular with Figure 3 On the contrary, there is basically no gap in the middle. Figure 3 The gaps in are only for a better understanding. Likewise, the processing zone 6 is guided in a spiral from the radially outer side to the radially inner side (or vice versa) to produce the coating layer 80. Figure 1 As can be seen in FIG. 8 , the surface 74 here comprises a coated radially outer section 82 and an uncoated radially inner section 84 .
[0057] Figure 4a The schematic cross-sectional view shows Figure 1 A laser deposition welding method for a similar component 70. Figure 1 The difference is that no Figure 1The processing head 20 described above. Alternatively, a plurality of injectors 46 (only two of which are shown here by way of example) are used here, by means of which the additional material 2 (in particular as a powder gas flow 4) is supplied directly to the laser beam 1. The injector 46 is shown here, for example, as a tube, in particular a hard metal tube. The tubes can be connected to the distributor component 42 by means of one, two or more supply lines 44, respectively. It is also possible that each injector 46 has its own distributor component 42, wherein the distributor component 42 can in turn be connected to the additional material conveyor 40. From Figure 4a It can also be seen in FIG. 8 that the laser beam 1 is now displaced with its laser beam axis LA, for example, in the X direction as the feed direction, and therefore also in this direction. This occurs during a rotation R of the component 70 about the axis of rotation 72 .
[0058] exist Figure 4a In addition, the exit angle of the injector 46 relative to the perpendicular to the respective surface 74 is less than 60°, which here coincides, for example, with the longitudinal axis LA of the laser beam 1. It has been shown that the surface waviness of the coating 80 welded thereby is particularly low.
[0059] Figure 4b A variant of the beam guidance of the laser beam 1 is shown, in which the laser beam axis LA of the laser beam 1 is at a favorable angle of incidence β relative to the surface 70, so that the laser beam 1 with its point of incidence falls on the surface 70 at the angle of incidence β. In this case, the angle of incidence β is, for example, 35°. The angle of incidence β can be achieved in particular by means of a processing head 20 which is arranged accordingly relative to the surface 70, in which the powder gas stream 4 can be guided, for example Figure 1 , or can be guided outside the processing head 20, so that only the laser beam 1 is guided in the processing head 20 or emitted from the processing head. Advantageously, the laser beam 1 that strikes the surface 74 at an angle of incidence β cannot be reflected back to the processing head 20 as laser light, but is deflected past the processing head. The waviness of the coating 80 is also further reduced.
[0060] Figure 5 1 shows a cross-sectional view of a portion of a component 70 during the execution of a conventional laser deposition welding method. Here, a coating track 86 having a track width B is applied to the surface 74. In the laser deposition welding methods known in the prior art, Figure 5 The next turn 8 (not shown) of the coating track 86 in Figure 5 It is applied to the right or radially inwardly of the component 70 beside the winding 8 shown. This leads to a high waviness of the coating 80 produced in this way, especially at high laser powers of the laser beam 1. Although this waviness can be reduced by subsequent grinding of the coating 80, the usable coating 80 is also reduced as a result.
[0061] Figure 6 A cross-sectional view of a portion of a component 70 during the implementation of a laser deposition welding method according to an exemplary embodiment of the present invention is shown. Along the track width B of the coating track 86, the same number of turns 8 are applied side by side and partially overlapping each other. In the present case, for example, in the track width B, approximately four turns 8 overlap each other. The number of turns 8 partially overlapping each other per track width B is determined here by the top view of the individual turns 8 per track width B. Therefore, only the part of the turns 8 visible on the surface is decisive.
[0062] As referenced later Figures 9 to 13 In detail, this overlap significantly reduces the surface waviness of the coating layer 80. Advantageously, a finishing grinding with a corresponding removal of the usable coating layer 80 can be avoided.
[0063] Figure 7 Again, a plan view of a portion of a component 70 from the prior art is shown, in which the windings 8 of a coating track 86 are applied with their track width B, which is defined by the focal diameter of the focusing lens of the laser beam 1 , wherein only one winding 8 is shown here.
[0064] on the contrary, Figure 8 The overlapping of a plurality of windings 8 of a coating track 86 in the region of a track width B is shown, as provided in a laser deposition welding method according to an exemplary embodiment of the invention.
[0065] Figures 9 to 13 A cross section of a component 70 with a coating layer 80 is shown, which differs by the number of windings 8 of the coating track 86 which (at least partially) partially overlap over the track width B.
[0066] Fig. 9 The result of the coating layer 80 partially overlapping 3.3 windings 8 arranged side by side along the track width B is shown, Fig.10 The result of coating layer 80 overlapping 3.7 windings 8 arranged side by side along the corresponding part of track width B is shown. As can be seen, relative to Figures 11 to 13 , even with this parameter selection, a relatively high waviness of the coating layer 80 still results.
[0067] Fig.11 The result is shown for 4.1 windings 8 of the coating layer 80 lying side by side and partially overlapping along the track width B. Fig.12 The result is shown with the coating layer 80 partially overlapping 4.7 turns 8 side by side along the track width B. And, Fig.13 The result is shown for a coating layer 80 partially overlapping 5.5 turns 8 side by side along the track width B. As can be seen, only a relatively low waviness of the coating layer 80 still results with this choice of parameters.
[0068] Accordingly, it has been shown that approximately four windings 8 partially overlapped side by side along the track width B produce generally such low waviness of the coating 80 that no compensating grinding is required or only minimal removal of the available coating 80 is required to achieve an optimal surface finish.
Claims
1. A laser deposition welding method for producing a coating (80) on a surface (74) of a component (70), wherein at least one coating track (86) having a predetermined track width (B) is produced on the surface (74) by applying an additive material (2), in particular a powdered additive material, along a helical or spiral processing path (88), wherein: The additive material (2) and the component (70) are heated along the processing trajectory (88) by means of a laser beam (1), so that when the additive material (2) impinges on the surface (74), at least one coating track (86) is generated, characterized in that at least two turns, in particular at least three turns (8) of the at least one coating track (86) at least partially overlap along the track width (B).
2. The laser deposition welding method according to claim 1, wherein: The respective at least four windings (8) of the coating track (86) at least partially overlap along the track width (B).
3. The laser deposition welding method according to claim 1 or 2, wherein: The windings (8) which at least partially overlap one another overlap one another by at least 20%, in particular by at least 40%, of the track width (B).
4. The laser deposition welding method according to any one of the preceding claims, wherein: During the production of the tooling layer (80), the number of windings (8) at least partially overlapping one another along the track width (B) is varied.
5. The laser deposition welding method according to any one of the preceding claims, wherein: On the windings (8) of the processing path (88) in the beginning and / or end region of its path width (B), further windings (8) of the at least one coating path (86) are produced.
6. The laser deposition welding method according to any one of the preceding claims, wherein: A height profile of the surface (74) coated with the at least one coating track (86) is generated by a measuring device (50).
7. The laser deposition welding method according to claim 6, wherein: The total thickness and / or waviness of the at least one coating track (86) on the surface (74) is determined based on the height profile and compared with predetermined limit values.
8. The laser deposition welding method according to any one of the preceding claims, wherein: The incident point of the laser beam (1) on the surface (74) moves along the surface (74) along the processing trajectory (88) at a relative speed of at least 20 m / min.
9. The laser deposition welding method according to any one of the preceding claims, wherein: The component (70) is designed to be rotationally symmetrical, in particular as a disk, and is rotated about an axis of rotation (72) during the production of the coating (80).
10. The laser deposition welding method according to any one of the preceding claims, wherein: At least one of the additive materials (2) is present as a powder before being melted by means of the laser beam (1).
11. The laser deposition welding method according to any one of the preceding claims, wherein: At least one of the additive materials (2) is supplied to the laser beam (1) by means of a conveying gas, wherein the conveying gas has in particular a relative atomic mass of at least 4 and / or a relative mass per mm 2 The cross-sectional area has a specific volume flow rate of at least 3.2 Nl / min.
12. The laser deposition welding method according to any one of the preceding claims, wherein: The coating layer (80) of the component (70) is manufactured in a direction from a relatively inner portion of the surface (74) to a relatively outer portion of the surface (74).
13. The laser deposition welding method according to any one of the preceding claims, wherein: The laser beam axis (LA) of the laser beam (1) is inclined at an angle of incidence (β) in the range of greater than 0° to 35° relative to the surface (74).
14. A component (70) having at least one surface (74) coated with a coating layer (80), wherein: The coating layer (80) is produced by means of a laser deposition welding method according to any one of the preceding claims.
15. A device (10) for performing the laser deposition welding method according to any one of claims 1 to 13, wherein: The device (10) has at least one laser (12) for generating a laser beam (1), wherein the device (10) comprises at least one additive material conveyor (40) for conveying at least one additive material (2) to the laser beam (1) at a distance from a surface (74) of a component (70).
Citation Information
Patent Citations
Process of treating a workpiece using a liquid jet guided laser beam
CN108025398A
Method used for superspeed laser cladding of end face of disc type part
CN111334789A
Regulated powder deposition welding process
DE102018130798A1
Device and method for post-processing layers applied by laser cladding
DE102020106822A1
Method for producing a protective coating on a brake side of a brake disc base body and method for producing a brake disc