Antibacterial composite material with slow release efficiency and preparation method thereof

By preparing antibacterial composite materials containing specific ingredients and using electrospinning technology, combined with sustained-release pain-repellent agents, the problems of insufficient antibacterial properties and lack of pain-relieving effects in human wounds are solved, and antibacterial composites are achieved The material's high-efficiency antibacterial and pain-relieving functions are both effective.

CN118892568APending Publication Date: 2024-11-05XIAMEN ETON GLOBAL MEDICAL EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310499225.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing antibacterial materials are weak in antibacterial properties when bandaged in human wounds and lack pain relief, resulting in discomfort in use and unable to meet medical needs.

Method used

A type of zinc salt, 2-aminoterephthalic acid, benzoic acid, nanomagnesium oxide, polyethylene glycol, polycaprolactone polyol, ZrCl4, lactide, tranexamic acid, 4-aminomethyl Composite materials of benzoic acid, aminopyrine, finacetin, caffeine and phenobarbital are prepared through specific process steps to prepare antibacterial composites with sustained release efficacy, combined with electrospinning technology to make dressings, and Apply sustained release pain relief agents on it.

Benefits of technology

It significantly improves the antibacterial properties and pain relief effects of antibacterial composite materials, reduces the discomfort during use, and meets the needs of dual functions of antibacterial and pain relief.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004213244350000101
    Figure BDA0004213244350000101
Patent Text Reader

Abstract

The invention discloses an antibacterial composite material with slow release efficiency and a preparation method thereof. The antibacterial composite material is prepared from the following raw materials: zinc salt, 2-aminoterephthalic acid, benzoic acid, concentrated hydrochloric acid, nano magnesium oxide, lanthanum chloride, polyethylene glycol, polycaprolactone polyol, polylactic acid, ZrCl4, lactide, tranexamic acid, 4-aminomethyl benzoic acid, aminopyrine, phenacetin, caffeine and phenobarbital. The antibacterial property of the antibacterial composite material can be effectively improved by adding the antibacterial agent into the antibacterial composite material dressing, and meanwhile, the pain relieving effect can be effectively improved by adding the prepared slow-release pain relieving agent mixture, so that the dressing is more beneficial to personnel use, and the discomfort of a patient during use is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of antibacterial composite materials, and in particular to an antibacterial composite material with sustained-release performance and a preparation method thereof. Background Art

[0002] Microorganisms in the form of bacteria, molds, etc. as pathogens can easily infect humans, animals and plants, cause diseases, and endanger human health and life. Antibacterial materials are an effective means to solve the above problems. In particular, materials used in medical treatment must have good antibacterial properties. In particular, when people are injured, antibacterial composite materials are needed to bandage the wound. Organic antibacterial materials are more commonly used in the prior art. This type of antibacterial material has weak antibacterial properties and can only stop bleeding when bandaging human wounds, but lacks analgesic effects. As a result, people still feel uncomfortable after bandaging, which cannot meet the use requirements. Based on the above situation, we propose an antibacterial composite material with sustained-release efficiency and a preparation method thereof. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes an antibacterial composite material with sustained-release efficacy and a preparation method thereof.

[0004] The invention provides an antibacterial composite material with sustained-release performance, which comprises the following raw materials in parts by weight: 1-2 parts of zinc salt, 2-3 parts of 2-aminoterephthalic acid, 1-2 parts of benzoic acid, 2-3 parts of concentrated hydrochloric acid, 1.5-4 parts of nano-magnesium oxide, 1-3 parts of lanthanum chloride, 1-2 parts of polyethylene glycol, 3-5 parts of polycaprolactone polyol, 1-3 parts of polylactic acid, 1-2 parts of ZrCl4, 18-20 parts of lactide, 10-15 parts of tranexamic acid, 8-10 parts of 4-aminomethylbenzoic acid, 13-15 parts of aminopyrine, 5-8 parts of phenacetin, 8-10 parts of caffeine and 10-12 parts of phenobarbital.

[0005] Preferably, the raw materials include the following parts by weight: 1 part of zinc salt, 2 parts of 2-aminoterephthalic acid, 1 part of benzoic acid, 2 parts of concentrated hydrochloric acid, 1.5 parts of nano-magnesium oxide, 1 part of lanthanum chloride, 1 part of polyethylene glycol, 3 parts of polycaprolactone polyol, 1 part of polylactic acid, 1 part of ZrCl4, 18 parts of lactide, 10 parts of tranexamic acid, 8 parts of 4-aminomethylbenzoic acid, 13 parts of aminopyrine, 5 parts of phenacetin, 8 parts of caffeine, and 10 parts of phenobarbital.

[0006] Preferably, the raw materials include the following parts by weight: 1.5 parts of zinc salt, 2.5 parts of 2-aminoterephthalic acid, 1.5 parts of benzoic acid, 2.5 parts of concentrated hydrochloric acid, 3 parts of nano-magnesium oxide, 2 parts of lanthanum chloride, 1.5 parts of polyethylene glycol, 4 parts of polycaprolactone polyol, 2 parts of polylactic acid, 1.5 parts of ZrCl4, 19 parts of lactide, 13 parts of tranexamic acid, 9 parts of 4-aminomethylbenzoic acid, 14 parts of aminopyrine, 6 parts of phenacetin, 9 parts of caffeine, and 11 parts of phenobarbital.

[0007] Preferably, the raw materials include the following parts by weight: 2 parts of zinc salt, 3 parts of 2-aminoterephthalic acid, 2 parts of benzoic acid, 3 parts of concentrated hydrochloric acid, 4 parts of nano magnesium oxide, 3 parts of lanthanum chloride, 2 parts of polyethylene glycol, 5 parts of polycaprolactone polyol, 3 parts of polylactic acid, 2 parts of ZrCl4, 20 parts of lactide, 15 parts of tranexamic acid, 7 parts of 4-aminomethylbenzoic acid, 15 parts of aminopyrine, 8 parts of phenacetin, 10 parts of caffeine, and 12 parts of phenobarbital.

[0008] The present invention also proposes a method for preparing an antibacterial composite material with sustained-release efficacy, comprising the following steps:

[0009] S1: 1.5-4 parts of nano magnesium oxide are selected and put into deionized water for dissolution, and then 1-3 parts of lanthanum chloride are added to the dissolved mixture, and after adding, the mixture is stirred and mixed with a stirrer, and after stirring and mixing, the mixture is poured into a heating pot and heated to 50-80° C.;

[0010] S2: pouring the heated solution mixture described in S1 into an acid-base indicator for acid adjustment, cooling and standing for 1-2 hours, then pouring the cooled material into a filter box for filtration, pouring it into a drying box for drying after filtration, and repeatedly grinding it after drying to obtain an antibacterial agent;

[0011] S3: 1-2 parts of zinc salt, 2-3 parts of 2-aminoterephthalic acid and 1-2 parts of benzoic acid are selected and poured into a mixing box at the same time for stirring and mixing, and after mixing, 2-3 parts of concentrated hydrochloric acid are added for ultrasonic dissolution to obtain a dissolved mixture;

[0012] S4: 1-2 parts of ZrCl4 are added to the mixture described in S3, and the mixture is dissolved again using an ultrasonic dissolver. After dissolution, the mixture is poured into a heating pot for heating treatment, and heated to 70-90° C. for hydrothermal reaction. After the hydrothermal reaction, 1 part of polyethylene glycol is added to the mixture for washing 3-5 times. After washing, the steps in S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material A;

[0013] S5: 18-20 parts of lactide, 10-15 parts of tranexamic acid and 8-10 parts of 4-aminomethylbenzoic acid are selected and put into a reactor at the same time for heating, and heated to 80-100° C. for hydrothermal reaction and dissolution, and after dissolution, 3-5 parts of polycaprolactone polyol are added for stirring and mixing, and an ultrasonic dissolver is used for dissolution and mixing, and after mixing, 1 part of ethylene glycol is used again for water washing 2-3 times, and after water washing, the steps in the above S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material B;

[0014] S6: 13-15 parts of aminopyrine, 5-8 parts of phenacetin, 8-10 parts of caffeine and 10-12 parts of phenobarbital are selected and poured into a reaction kettle at the same time, and an appropriate amount of deionized water is added and dissolved and mixed using an ultrasonic dissolver, and after mixing, a thermal reaction is performed by heating for 30-50 minutes to obtain a sustained-release analgesic drug mixture;

[0015] S7: adding the antibacterial agent described in S2, the composite material A described in S4, and the composite material B described in S5 into a stirring mixing box at the same time for stirring and mixing, adding 1-3 parts of polylactic acid after stirring and mixing evenly, continuing to stir and mix, and after mixing, using electrospinning technology to prepare an antibacterial composite material dressing;

[0016] S8: Apply the sustained-release analgesic drug mixture described in S6 to the antibacterial composite dressing described in S7, apply it evenly, and then put it into a drying oven for drying, so as to obtain an antibacterial composite material with sustained-release efficacy.

[0017] Preferably, in S1, nano magnesium oxide is dissolved in ionized water by ultrasonic dispersion.

[0018] Preferably, in S3, the zinc salt is one or more of zinc acetate, zinc nitrate, zinc sulfate and zinc chloride.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention can effectively improve the antibacterial properties of the antibacterial composite material by adding an antibacterial agent to the antibacterial composite material dressing, and can effectively improve the analgesic effect by adding the prepared sustained-release analgesic drug mixture, which is more conducive to personnel use and reduces the discomfort of patients when using it. DETAILED DESCRIPTION

[0021] The present invention will be further explained below in conjunction with specific embodiments.

[0022] Embodiment 1

[0023] This embodiment proposes an antibacterial composite material with sustained-release performance, comprising the following raw materials in parts by weight: 1 part of zinc salt, 2 parts of 2-aminoterephthalic acid, 1 part of benzoic acid, 2 parts of concentrated hydrochloric acid, 1.5 parts of nano-magnesium oxide, 1 part of lanthanum chloride, 1 part of polyethylene glycol, 3 parts of polycaprolactone polyol, 1 part of polylactic acid, 1 part of ZrCl4, 18 parts of lactide, 10 parts of tranexamic acid, 8 parts of 4-aminomethylbenzoic acid, 13 parts of aminopyrine, 5 parts of phenacetin, 8 parts of caffeine, and 10 parts of phenobarbital.

[0024] This embodiment also proposes a method for preparing an antibacterial composite material with sustained-release performance, comprising the following steps:

[0025] S1: 1.5 parts of nano-magnesium oxide are selected and put into deionized water for dissolution, and then 1 part of lanthanum chloride is added to the dissolved mixture, and after adding, the mixture is stirred and mixed using a stirrer, and after stirring and mixing, the mixture is poured into a heating pot and heated to 50° C., wherein the nano-magnesium oxide is dissolved in the deionized water by ultrasonic dispersion;

[0026] S2: pouring the heated solution mixture described in S1 into an acid-base indicator for acid adjustment, cooling and standing for 1 hour, then pouring the cooled material into a filter box for filtration, pouring it into a drying box for drying after filtration, and repeatedly grinding it after drying to obtain an antibacterial agent;

[0027] S3: Select 1 part of zinc salt, 2 parts of 2-aminoterephthalic acid and 1 part of benzoic acid, pour them into a mixing box at the same time, stir and mix, add 2 parts of concentrated hydrochloric acid after mixing, ultrasonically dissolve, and obtain a dissolved mixture, wherein the zinc salt is one or more of zinc acetate, zinc nitrate, zinc sulfate and zinc chloride;

[0028] S4: Select 1 part of ZrCl4 and add it to the mixture described in S3, and dissolve it again using an ultrasonic dissolver. After dissolution, pour it into a heating pot for heating treatment, heat it to 70°C for hydrothermal reaction, and after the hydrothermal reaction, add 1 part of polyethylene glycol to the mixture and wash it with water 3 times. After washing with water, repeat the steps in S2 above, filter, dry and repeatedly grind the mixture to obtain a composite material A;

[0029] S5: 18 parts of lactide, 10 parts of tranexamic acid and 8 parts of 4-aminomethylbenzoic acid are selected and put into a reactor at the same time for heating, and heated to 80° C. for hydrothermal reaction and dissolution. After dissolution, 3 parts of polycaprolactone polyol are added for stirring and mixing, and an ultrasonic dissolver is used for dissolution and mixing. After mixing, 1 part of ethylene glycol is used for water washing twice again. After water washing, the steps in S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material B;

[0030] S6: 13 parts of aminopyrine, 5 parts of phenacetin, 8 parts of caffeine and 10 parts of phenobarbital are selected and poured into a reactor at the same time, and an appropriate amount of deionized water is added to dissolve and mix using an ultrasonic dissolver, and after mixing, a thermal reaction is performed by heating for 30 minutes to obtain a sustained-release analgesic drug mixture;

[0031] S7: adding the antibacterial agent described in S2, the composite material A described in S4, and the composite material B described in S5 into a stirring mixing box at the same time for stirring and mixing, adding 1 part of polylactic acid after stirring and mixing evenly, continuing to stir and mix, and after mixing, using electrospinning technology to prepare an antibacterial composite material dressing;

[0032] S8: Apply the sustained-release analgesic drug mixture described in S6 to the antibacterial composite dressing described in S7, apply it evenly, and then put it into a drying oven for drying, so as to obtain an antibacterial composite material with sustained-release efficacy.

[0033] Embodiment 2

[0034] This embodiment provides an antibacterial composite material with sustained-release performance, comprising the following raw materials in parts by weight: 1.5 parts of zinc salt, 2.5 parts of 2-aminoterephthalic acid, 1.5 parts of benzoic acid, 2.5 parts of concentrated hydrochloric acid, 3 parts of nano-magnesium oxide, 2 parts of lanthanum chloride, 1.5 parts of polyethylene glycol, 4 parts of polycaprolactone polyol, 2 parts of polylactic acid, 1.5 parts of ZrCl4, 19 parts of lactide, 13 parts of tranexamic acid, 9 parts of 4-aminomethylbenzoic acid, 14 parts of aminopyrine, 6 parts of phenacetin, 9 parts of caffeine, and 11 parts of phenobarbital;

[0035] This embodiment also proposes a method for preparing an antibacterial composite material with sustained-release performance, comprising the following steps:

[0036] S1: Select 3 parts of nano-magnesium oxide and put them into deionized water for dissolution, then add 2 parts of lanthanum chloride to the dissolved mixture, stir and mix them with a stirrer, pour them into a heating pot and heat them to 70° C., wherein the nano-magnesium oxide is dissolved in the deionized water by ultrasonic dispersion;

[0037] S2: pouring the heated solution mixture described in S1 into an acid-base indicator for acid adjustment, cooling and standing for 1.5 hours, then pouring the cooled material into a filter box for filtration, pouring it into a drying box for drying after filtration, and repeatedly grinding it after drying to obtain an antibacterial agent;

[0038] S3: 1.5 parts of zinc salt, 2.5 parts of 2-aminoterephthalic acid and 1.5 parts of benzoic acid are selected and poured into a mixing box at the same time for stirring and mixing, and after mixing, 2.5 parts of concentrated hydrochloric acid are added for ultrasonic dissolution to obtain a dissolved mixture, wherein the zinc salt is one or more of zinc acetate, zinc nitrate, zinc sulfate and zinc chloride;

[0039] S4: 1.5 parts of ZrCl4 are selected and added to the mixture described in S3, and the mixture is dissolved again using an ultrasonic dissolver. After dissolution, the mixture is poured into a heating pot for heating treatment, and heated to 80° C. for hydrothermal reaction. After the hydrothermal reaction, 1 part of polyethylene glycol is added to the mixture and the mixture is washed with water 4 times. After washing with water, the steps in S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material A;

[0040] S5: 19 parts of lactide, 13 parts of tranexamic acid and 9 parts of 4-aminomethylbenzoic acid are selected and put into a reactor at the same time for heating, and heated to 90° C. for hydrothermal reaction dissolution, and after dissolution, 4 parts of polycaprolactone polyol are added for stirring and mixing, and an ultrasonic dissolver is used for dissolution and mixing, and after mixing, 1 part of ethylene glycol is used for water washing twice again, and after water washing, the steps in S2 are repeated, and the mixture is filtered, dried and repeatedly ground to obtain a composite material B;

[0041] S6: 14 parts of aminopyrine, 6 parts of phenacetin, 9 parts of caffeine and 11 parts of phenobarbital are selected and poured into a reactor at the same time, and an appropriate amount of deionized water is added to dissolve and mix using an ultrasonic dissolver, and after mixing, a thermal reaction is performed by heating for 40 minutes to obtain a sustained-release analgesic drug mixture;

[0042] S7: adding the antibacterial agent described in S2, the composite material A described in S4, and the composite material B described in S5 into a stirring mixing box at the same time for stirring and mixing, adding 2 parts of polylactic acid after stirring and mixing evenly, continuing to stir and mix, and after mixing, using electrospinning technology to prepare an antibacterial composite dressing;

[0043] S8: Apply the sustained-release analgesic drug mixture described in S6 to the antibacterial composite dressing described in S7, apply it evenly, and then put it into a drying oven for drying, so as to obtain an antibacterial composite material with sustained-release efficacy.

[0044] Embodiment 3

[0045] This embodiment provides an antibacterial composite material with sustained-release performance, comprising the following raw materials in parts by weight: 2 parts of zinc salt, 3 parts of 2-aminoterephthalic acid, 2 parts of benzoic acid, 3 parts of concentrated hydrochloric acid, 4 parts of nano-magnesium oxide, 3 parts of lanthanum chloride, 2 parts of polyethylene glycol, 5 parts of polycaprolactone polyol, 3 parts of polylactic acid, 2 parts of ZrCl4, 20 parts of lactide, 15 parts of tranexamic acid, 7 parts of 4-aminomethylbenzoic acid, 15 parts of aminopyrine, 8 parts of phenacetin, 10 parts of caffeine, and 12 parts of phenobarbital;

[0046] This embodiment also proposes a method for preparing an antibacterial composite material with sustained-release performance, comprising the following steps:

[0047] S1: Select 4 parts of nano-magnesium oxide and put them into deionized water for dissolution, then add 3 parts of lanthanum chloride to the dissolved mixture, stir and mix them with a stirrer, pour them into a heating pot and heat them to 80° C., wherein the nano-magnesium oxide is dissolved in the deionized water by ultrasonic dispersion;

[0048] S2: pouring the heated solution mixture described in S1 into an acid-base indicator for acid adjustment, cooling and standing for 2 hours, then pouring the cooled material into a filter box for filtration, pouring it into a drying box for drying after filtration, and repeatedly grinding it after drying to obtain an antibacterial agent;

[0049] S3: Select 2 parts of zinc salt, 3 parts of 2-aminoterephthalic acid and 2 parts of benzoic acid, pour them into a mixing box at the same time, stir and mix, add 3 parts of concentrated hydrochloric acid after mixing, ultrasonically dissolve, and obtain a dissolved mixture, wherein the zinc salt is one or more of zinc acetate, zinc nitrate, zinc sulfate and zinc chloride;

[0050] S4: Select 2 parts of ZrCl4 and add them to the mixture described in S3, and use an ultrasonic dissolver to dissolve them again. After dissolution, pour them into a heating pot for heating treatment, heat them to 90°C for hydrothermal reaction, and after the hydrothermal reaction, add 1 part of polyethylene glycol to the mixture and wash them with water 5 times. After washing with water, repeat the steps in S2 above, filter, dry and repeatedly grind the mixture to obtain a composite material A;

[0051] S5: 20 parts of lactide, 15 parts of tranexamic acid and 10 parts of 4-aminomethylbenzoic acid are selected and put into a reactor at the same time for heating, and heated to 100° C. for hydrothermal reaction dissolution, and after dissolution, 5 parts of polycaprolactone polyol are added for stirring and mixing, and an ultrasonic dissolver is used for dissolution and mixing, and after mixing, 1 part of ethylene glycol is used again for water washing 3 times, and after water washing, the steps in the above S2 are repeated, and the mixture is filtered, dried and repeatedly ground to obtain a composite material B;

[0052] S6: 15 parts of aminopyrine, 8 parts of phenacetin, 10 parts of caffeine and 12 parts of phenobarbital are selected and poured into a reactor at the same time, and an appropriate amount of deionized water is added to dissolve and mix using an ultrasonic dissolver, and after mixing, a thermal reaction is performed for 50 minutes to obtain a sustained-release analgesic drug mixture;

[0053] S7: adding the antibacterial agent described in S2, the composite material A described in S4, and the composite material B described in S5 into a stirring mixing box at the same time for stirring and mixing, adding 3 parts of polylactic acid after stirring and mixing evenly, continuing to stir and mix, and after mixing, using electrospinning technology to prepare an antibacterial composite dressing;

[0054] S8: Apply the sustained-release analgesic drug mixture described in S6 to the antibacterial composite dressing described in S7, apply it evenly, and then put it into a drying oven for drying, so as to obtain an antibacterial composite material with sustained-release efficacy.

[0055] The experimental data of the antibacterial composite materials prepared in Examples 1 to 3 are compared with conventional antibacterial composite materials as shown in the following table:

[0056]

[0057] It can be seen from the above table that the antibacterial performance and analgesic performance of the antibacterial composite material with sustained-release efficiency proposed by the present invention are significantly improved, and implementation 2 is the best embodiment.

[0058] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An antibacterial composite material with sustained-release performance, characterized in that: The invention comprises the following raw materials in parts by weight: 1-2 parts of zinc salt, 2-3 parts of 2-aminoterephthalic acid, 1-2 parts of benzoic acid, 2-3 parts of concentrated hydrochloric acid, 1.5-4 parts of nano magnesium oxide, 1-3 parts of lanthanum chloride, 1-2 parts of polyethylene glycol, 3-5 parts of polycaprolactone polyol, 1-3 parts of polylactic acid, 1-2 parts of ZrCl4, 18-20 parts of lactide, 10-15 parts of tranexamic acid, 8-10 parts of 4-aminomethylbenzoic acid, 13-15 parts of aminopyrine, 5-8 parts of phenacetin, 8-10 parts of caffeine and 10-12 parts of phenobarbital.

2. The antibacterial composite material with sustained release performance according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 1 part of zinc salt, 2 parts of 2-aminoterephthalic acid, 1 part of benzoic acid, 2 parts of concentrated hydrochloric acid, 1.5 parts of nano magnesium oxide, 1 part of lanthanum chloride, 1 part of polyethylene glycol, 3 parts of polycaprolactone polyol, 1 part of polylactic acid, 1 part of ZrCl4, 18 parts of lactide, 10 parts of tranexamic acid, 8 parts of 4-aminomethylbenzoic acid, 13 parts of aminopyrine, 5 parts of phenacetin, 8 parts of caffeine and 10 parts of phenobarbital.

3. The antibacterial composite material with sustained-release performance according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 1.5 parts of zinc salt, 2.5 parts of 2-aminoterephthalic acid, 1.5 parts of benzoic acid, 2.5 parts of concentrated hydrochloric acid, 3 parts of nano magnesium oxide, 2 parts of lanthanum chloride, 1.5 parts of polyethylene glycol, 4 parts of polycaprolactone polyol, 2 parts of polylactic acid, 1.5 parts of ZrCl4, 19 parts of lactide, 13 parts of tranexamic acid, 9 parts of 4-aminomethylbenzoic acid, 14 parts of aminopyrine, 6 parts of phenacetin, 9 parts of caffeine and 11 parts of phenobarbital.

4. The antibacterial composite material with sustained-release performance according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 2 parts of zinc salt, 3 parts of 2-aminoterephthalic acid, 2 parts of benzoic acid, 3 parts of concentrated hydrochloric acid, 4 parts of nano magnesium oxide, 3 parts of lanthanum chloride, 2 parts of polyethylene glycol, 5 parts of polycaprolactone polyol, 3 parts of polylactic acid, 2 parts of ZrCl4, 20 parts of lactide, 15 parts of tranexamic acid, 7 parts of 4-aminomethylbenzoic acid, 15 parts of aminopyrine, 8 parts of phenacetin, 10 parts of caffeine and 12 parts of phenobarbital.

5. The method for preparing an antibacterial composite material with sustained-release performance according to claim 1, characterized in that: The following steps are involved: S1: 1.5-4 parts of nano magnesium oxide are selected and put into deionized water for dissolution, and then 1-3 parts of lanthanum chloride are added to the dissolved mixture, and after adding, the mixture is stirred and mixed with a stirrer, and after stirring and mixing, the mixture is poured into a heating pot and heated to 50-80° C.; S2: pouring the heated solution mixture described in S1 into an acid-base indicator for acid adjustment, cooling and standing for 1-2 hours, then pouring the cooled material into a filter box for filtration, pouring it into a drying box for drying after filtration, and repeatedly grinding it after drying to obtain an antibacterial agent; S3: 1-2 parts of zinc salt, 2-3 parts of 2-aminoterephthalic acid and 1-2 parts of benzoic acid are selected and poured into a mixing box at the same time for stirring and mixing, and after mixing, 2-3 parts of concentrated hydrochloric acid are added for ultrasonic dissolution to obtain a dissolved mixture; S4: 1-2 parts of ZrCl4 are added to the mixture described in S3, and the mixture is dissolved again using an ultrasonic dissolver. After dissolution, the mixture is poured into a heating pot for heating treatment, and heated to 70-90° C. for hydrothermal reaction. After the hydrothermal reaction, 1 part of polyethylene glycol is added to the mixture for washing 3-5 times. After washing, the steps in S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material A; S5: 18-20 parts of lactide, 10-15 parts of tranexamic acid and 8-10 parts of 4-aminomethylbenzoic acid are selected and put into a reactor at the same time for heating, and heated to 80-100° C. for hydrothermal reaction and dissolution, and after dissolution, 3-5 parts of polycaprolactone polyol are added for stirring and mixing, and an ultrasonic dissolver is used for dissolution and mixing, and after mixing, 1 part of ethylene glycol is used again for water washing 2-3 times, and after water washing, the steps in the above S2 are repeated to filter, dry and repeatedly grind the mixture to obtain a composite material B; S6: 13-15 parts of aminopyrine, 5-8 parts of phenacetin, 8-10 parts of caffeine and 10-12 parts of phenobarbital are selected and poured into a reaction kettle at the same time, and an appropriate amount of deionized water is added and dissolved and mixed using an ultrasonic dissolver, and after mixing, a thermal reaction is performed by heating for 30-50 minutes to obtain a sustained-release analgesic drug mixture; S7: adding the antibacterial agent described in S2, the composite material A described in S4, and the composite material B described in S5 into a stirring mixing box at the same time for stirring and mixing, adding 1-3 parts of polylactic acid after stirring and mixing evenly, continuing to stir and mix, and after mixing, using electrospinning technology to prepare an antibacterial composite material dressing; S8: Apply the sustained-release analgesic drug mixture described in S6 to the antibacterial composite dressing described in S7, apply it evenly, and then put it into a drying oven for drying, so as to obtain an antibacterial composite material with sustained-release efficacy.

6. The method for preparing an antibacterial composite material with sustained-release performance according to claim 5, characterized in that: In S1, nano magnesium oxide is dissolved in ionized water by ultrasonic dispersion.

7. The method for preparing an antibacterial composite material with sustained-release performance according to claim 5, characterized in that: In S3, the zinc salt is one or more of zinc acetate, zinc nitrate, zinc sulfate and zinc chloride.