Composite membrane based on metal organic framework material as well as preparation method and application of composite membrane

By combining graphene oxide film with metal organic framework materials, a dense and defect-free composite film is constructed, which solves the problems of low efficiency of traditional water treatment methods and limited material applications, and achieves the effect of efficiently intercepting organic dyes, and demonstrates the Good application prospects in the field of water treatment.

CN118892749APending Publication Date: 2024-11-05ZHEJIANG NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073216.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional water treatment methods are difficult to meet the requirements of high efficiency and environmental protection, and metal organic frame materials mainly exist in powder form, which limits their application in the field of membrane separation.

Method used

By combining the graphene oxide film with the metal organic framework material, the rich oxygen-containing groups on the surface of the graphene oxide film are used to enrich zirconium ions, and in-situ growth method is used to construct a dense and defect-free graphene oxide/metal organic framework material composite film. , achieving high porosity and high water permeability, while maintaining the retention performance of dye molecules.

Benefits of technology

It achieves high permeability and selectivity, can efficiently intercept organic dyes in wastewater, has a simple preparation process and low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892749A_ABST
    Figure CN118892749A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of membrane separation, and particularly relates to a composite membrane based on a metal organic framework material as well as a preparation method and application of the composite membrane. The preparation method of the composite membrane based on the metal organic framework material comprises the following steps: performing suction filtration on a graphene oxide dispersion liquid to a substrate membrane to obtain a graphene oxide membrane; soaking the graphene oxide film in a zirconium ion-containing solution to obtain a zirconium ion / graphene oxide film; and soaking the zirconium ion / graphene oxide film in a precursor solution of a metal organic framework material, and carrying out a heating reaction to prepare the composite film, wherein the precursor solution is a mixed solution containing an organic ligand and the zirconium ion-containing solution. The preparation method has the advantages of simplicity in operation, mild reaction conditions, wide application and the like, and the prepared composite membrane can be applied to separation of organic dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of membrane separation, and in particular relates to a composite membrane based on a metal organic framework material and a preparation method and application thereof. Background Art

[0002] Traditional water treatment methods can no longer meet the requirements of high efficiency and environmental protection. Membrane separation, as an emerging energy-saving and environmentally friendly separation technology, has the advantages of high efficiency, energy saving and continuous operation, and is widely used in the separation field. Metal-organic framework (MOF) materials have shown great potential in the field of water treatment due to their unique structure and high specific surface area. However, MOF mainly exists in the form of powder, which greatly limits the practical application of MOF. Therefore, it is necessary to carry out research on MOF preparation technology based on separation membranes to realize the preparation and application of its nanoscale thin films.

[0003] To this end, the present invention is proposed. Summary of the invention

[0004] The main purpose of the present invention is to provide a composite membrane based on metal organic framework materials and a preparation method and application thereof. The preparation method of the present invention is simple to operate and has mild reaction conditions. The prepared composite membrane has a large flux and is dense and defect-free.

[0005] In order to achieve the above objectives, the present invention provides the following technical solutions.

[0006] In a first aspect, the present invention provides a method for preparing a composite membrane based on a metal organic framework material, which comprises the following steps:

[0007] The graphene oxide dispersion is filtered onto the substrate membrane to obtain a graphene oxide membrane;

[0008] Immersing the graphene oxide film in a zirconium ion-containing solution to obtain a zirconium ion / graphene oxide film;

[0009] Immersing the zirconium ion / graphene oxide film in a precursor solution of a metal organic framework material and performing a heating reaction to obtain the composite film;

[0010] Wherein, the precursor solution is a mixed solution containing an organic ligand and the zirconium ion-containing solution.

[0011] In some embodiments of the present invention, the zirconium ion-containing solution is an aqueous solution containing zirconium ions. For example, the aqueous solution containing zirconium ions can be a zirconium chloride solution.

[0012] In some embodiments of the present invention, the concentration of the zirconium ion-containing solution is 0.95 mol / L to 1.05 mol / L.

[0013] In some embodiments of the present invention, the ratio of solute to solvent in the ZrCl4 solution is 1:4.3, that is, the mass fraction of the ZrCl4 solution is 18.9%.

[0014] In some embodiments of the present invention, the organic ligand is L-aspartic acid.

[0015] In some embodiments of the present invention, in the precursor solution, the mass ratio of the organic ligand to the zirconium ion-containing solution is 1:(0.8-1.2). For example, the mass ratio may be one of 1:0.8, 1:0.9, 1:1.0, 1:1.1, 1:1.2 or any value satisfying the above range.

[0016] In some embodiments of the present invention, the molar ratio of the L-aspartic acid to the ZrCl4 is 21:10.

[0017] In some embodiments of the present invention, the concentration of the graphene oxide dispersion is 0.001 mg / mL to 0.005 mg / mL. For example, the concentration of the graphene oxide dispersion can be one of 0.001 mg / mL, 0.002 mg / mL, 0.003 mg / mL, 0.004 mg / mL, 0.005 mg / mL, or any value satisfying the above range.

[0018] In some embodiments of the present invention, the volume of the graphene oxide dispersion is 10 mL to 20 mL. For example, the amount of the graphene oxide dispersion can be one of 10 mL, 11 mL, 12 mL, 13 mL, 14 mL, 15 mL, 16 mL, 17 mL, 18 mL, 19 mL, 20 mL or any value satisfying the above range.

[0019] In some embodiments of the present invention, the immersion time of the graphene oxide film in the zirconium ion-containing solution is 16 hours to 24 hours. For example, the immersion time can be one of 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, or any value that satisfies the above range.

[0020] In some embodiments of the present invention, the temperature of the heating reaction is 118°C to 122°C, and the time is 0.75h to 1.25h. For example, the heating temperature can be one of 118°C, 119°C, 120°C, 121°C, 122°C, or any value satisfying the above range. The heating time can be one of 0.75h, 0.80h, 0.85h, 0.90h, 0.95h, 1.0h, 1.1h, 1.15h, 1.20h, 1.25h, or any value satisfying the above range.

[0021] In some embodiments of the present invention, the base film includes one of a cellulose acetate film, a nylon film, and a polytetrafluoroethylene film.

[0022] In some embodiments of the present invention, the preparation method further comprises drying the prepared composite nanofiltration membrane.

[0023] In some embodiments of the present invention, the drying temperature is 20°C to 30°C, and the drying time is 18h to 24h. For example, the drying temperature can be one of 20°C, 25°C, 30°C, or any value within the above range. The drying time can be one of 18h, 19h, 20h, 21h, 22h, 23h, 24h, or any value within the above range.

[0024] In a second aspect, the present invention provides a composite membrane based on a metal organic framework material, wherein the composite membrane is prepared by the preparation method described in the first aspect.

[0025] The third aspect of the present invention provides an application of the metal organic framework material based composite membrane described in the first aspect or the metal organic framework material based composite membrane prepared by the preparation method described in the second aspect in water purification.

[0026] Compared with the prior art, the present invention achieves the following technical effects:

[0027] 1) The present invention forms a composite membrane with excellent performance by combining metal organic framework materials with graphene oxide. On the one hand, using graphene oxide membrane as a substrate, the rich oxygen-containing groups on the surface of the graphene oxide membrane can enrich the zirconium ions in the solution, providing a large number of nucleation sites for the subsequent growth of metal organic framework materials, and constructing a dense and defect-free graphene oxide membrane / metal organic framework material composite membrane through an in-situ growth method; on the other hand, the high porosity of the metal organic framework material significantly improves the water permeability of the graphene oxide membrane / metal organic framework material composite membrane, but the retention performance of dye molecules is basically maintained, effectively breaking through the problem of mutual restriction between membrane permeability and selectivity. Combining the above two aspects, the graphene oxide / metal organic framework material composite membrane has high permeability and selectivity, and can be used for efficient retention of organic dyes in wastewater.

[0028] 2) In the preparation method provided by the present invention, the graphene oxide membrane can be quickly prepared by vacuum filtration, and the growth process of the metal organic framework material is only carried out in water solvent and at a relatively low temperature. The preparation process of the membrane is simple, does not require a large amount of organic solvent, is low in cost, and can be applied to large-scale industrial production.

[0029] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:

[0031] Figure 1 This is a picture of the water contact angle of the graphene oxide / MOF composite film prepared in Example 1;

[0032] Figure 2 is a scanning electron microscope image of the graphene oxide / MOF composite film obtained in Example 1;

[0033] Figure 3 The retention performance of the graphene oxide / MOF composite membrane prepared in Example 1;

[0034] Figure 4 is a scanning electron microscope image of the graphene oxide / MOF composite film obtained in Example 2;

[0035] Figure 5 is a scanning electron microscope image of the graphene oxide / MOF composite film obtained in Comparative Example 1;

[0036] Figure 6 This is a scanning electron microscope image of the graphene oxide / MOF composite film prepared in Comparative Example 2. DETAILED DESCRIPTION

[0037] The exemplary embodiments of the present invention will be described in more detail below with reference to specific embodiments. It should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" in the specification and claims of the present invention and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0039] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0040] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this document generally indicates that the associated objects before and after are in an "or" relationship.

[0041] In the description of the embodiments of the present invention, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0042] MOF is a porous crystalline framework composed of metal cations or metal clusters and organic ligands. It has multifunctional properties such as high surface area, adjustable pore size, and abundant active sites, making it one of the ideal membrane materials. In situ growth is one of the most commonly used methods for preparing MOF membranes. Usually, metal ions are fixed on the interface layer and then used for the nucleation growth of MOF membranes. However, the high crystallinity of MOF usually causes intercrystalline defects or cracks between adjacent crystals, which leads to a significant decrease in the selectivity of MOF membranes.

[0043] As a typical two-dimensional sheet material, graphene oxide contains a large number of oxygen-containing groups on its surface, which has good affinity for metal ions and can provide a large number of binding sites for them. Using graphene oxide / metal ion composite layer as a substrate is expected to induce the uniform growth of MOF film and obtain a dense and defect-free graphene oxide / MOF composite film.

[0044] To this end, the present invention aims to solve the problem that intercrystalline defects or cracks are easily generated in the preparation method of MOF composite membrane, which limits the selectivity of MOF membrane, and provides a preparation method of dense and defect-free graphene oxide / MOF composite membrane by in-situ growth of MOF using ultra-thin graphene oxide film as a substrate.

[0045] The method for preparing a composite membrane based on a metal organic framework material in the present invention is carried out according to the following steps.

[0046] 1) Preparation of graphene oxide film.

[0047] Prepare graphene oxide dispersion: measure 5 μL to 50 μL of 1 mg / mL graphene oxide solution into a beaker, dilute to 10 mL to 50 mL with a dispersion solvent, and perform ultrasound to assist dispersion for 5 min to 15 min to obtain a graphene oxide dispersion.

[0048] The graphene oxide dispersion is filtered by using a base membrane to obtain a graphene oxide membrane.

[0049] In some embodiments of the present invention, the dispersion solvent may be deionized water.

[0050] In some embodiments of the present invention, the graphene oxide dispersion is filtered on the substrate membrane by vacuum filtration. For example, the vacuum degree may be 1 bar.

[0051] In some embodiments of the present invention, the base film includes but is not limited to cellulose acetate film, nylon film, polytetrafluoroethylene film.

[0052] 2) Preparation of zirconium ion / graphene oxide membrane.

[0053] The graphene oxide film is immersed in a precursor metal solution of a metal organic framework material MIP-202 (Zr), namely a zirconium ion solution, for 16 to 24 hours, and then taken out to obtain a zirconium ion / graphene oxide film.

[0054] In some embodiments of the present invention, the precursor metal solution of the metal organic framework material may be an aqueous solution containing zirconium ions.

[0055] Exemplarily, the solvent in the aqueous solution containing zirconium ions is deionized water, such as zirconium chloride (ZrCl 4 ) solution.

[0056] In some embodiments of the present invention, the amount of ZrCl4 is 1 g to 5 g, for example, 1 g, 2 g, 3 g, 4 g, 5 g or any value that satisfies the above range. The mass ratio of solute to solvent in the ZrCl4 solution is 1:4.3.

[0057] In some embodiments of the present invention, the concentration of the precursor metal solution is 0.95 mol / L to 1.05 mol / L.

[0058] 3) Preparing a precursor solution of a metal organic framework material.

[0059] The remaining precursor metal solution in step 2) is transferred to a container, such as a sealed reaction container such as a blue-capped bottle or a reactor, and the organic ligand is added and stirred evenly until completely dissolved to obtain a precursor solution of a metal organic framework material.

[0060] In some embodiments of the present invention, the organic ligand is L-aspartic acid.

[0061] In some embodiments of the present invention, the mass ratio of the organic ligand to the precursor metal solution is 1:(0.8-1.2). For example, the mass ratio may be one of 1:0.8, 1:0.9, 1:1.0, 1:1.1, 1:1.2 or any value satisfying the above range.

[0062] In some embodiments of the present invention, the molar ratio of L-aspartic acid to ZrCl4 is 21:10.

[0063] In some embodiments of the present invention, the stirring may be magnetic stirring, and the rotation speed is 300 rpm to 600 rpm, for example, 300 rpm, 400 rpm, 500 rpm, 600 rpm or any value satisfying the above range.

[0064] 4) Preparation of composite membrane.

[0065] The zirconium ion / graphene oxide film is immersed in a precursor solution of a metal organic framework material and heated to react to obtain a composite film.

[0066] In some embodiments of the present invention, the heating temperature is 118° C. to 122° C., and the heating time is 0.75 h to 1.25 h.

[0067] In some embodiments of the present invention, the heating reaction can be performed in a forced air oven.

[0068] 5) Drying treatment.

[0069] The composite film obtained after the heating reaction is completed is taken out and dried at a temperature of 20°C to 30°C for 18h to 24h.

[0070] In some embodiments of the present invention, a graphene oxide film is first prepared by a vacuum-assisted self-assembly method, and the graphene oxide film is immersed in a ZrCl4 solution. After the immersion is completed, a zirconium ion / graphene oxide film is obtained; then the ZrCl4 solution is transferred to a blue-capped bottle, and L-aspartic acid is added to obtain a mixed solution; thereafter, the zirconium ion / graphene oxide film is immersed in the above-mentioned mixed solution, reacted at high temperature for a period of time, and after the reaction is completed, it is taken out and placed at room temperature for drying to obtain a composite film based on zirconium metal organic framework material.

[0071] The present invention also provides a composite membrane based on a metal organic framework material prepared by the above method.

[0072] The composite membrane provided in the present invention combines the high specific surface area of ​​MOF materials with the excellent mechanical properties and chemical stability of graphene oxide materials, and shows good application prospects in the field of water treatment. The composite membrane can be used for intercepting and removing organic dyes in wastewater.

[0073] The chemical reagents used in the specification and examples of the present invention include any conventional models or types in the art, and the present invention does not impose any special limiting requirements.

[0074] Example 1

[0075] (1) A 1.0 mg / mL graphene oxide solution was prepared, 25 μL of the graphene oxide solution was taken and diluted to 10 mL to obtain a 0.0025 mg / mL graphene oxide dispersion, and the graphene oxide dispersion was filtered using a nylon membrane to obtain a graphene oxide membrane.

[0076] (2) The graphene oxide film was immersed in a ZrCl4 solution (0.95 mol / L, 10 mL) for 24 h. After the immersion was completed, the zirconium ion / graphene oxide film was taken out to obtain the zirconium ion / graphene oxide film.

[0077] (3) The remaining solution in step (2) was transferred to a 100 mL blue-capped bottle. L-aspartic acid (2.80 g, 21 mmol) was then added to the solution and stirred until completely dissolved to obtain a mixed solution.

[0078] (4) Then, the zirconium ion / graphene oxide film was immersed in the above mixed solution and reacted at 120° C. for 1.25 h. After the reaction was completed, the film was taken out and dried at room temperature of 25° C. for 20 h.

[0079] (5) After the preparation is completed, the wettability, membrane surface morphology, etc. of the above-mentioned graphene oxide / MOF composite membrane are characterized, and a separation test is performed.

[0080] Determination of membrane surface wettability: The surface hydrophilicity and hydrophobicity of the graphene oxide / MOF composite membrane were determined by a contact angle meter. During the measurement, the sample was first fixed on a glass slide adhered with double-sided tape, and then placed directly below the micro-syringe. The droplet volume was set to 5.0 μL. After the droplets on the sample surface stabilized, the camera of the instrument was used to take pictures and record them. The contact angle values ​​were calculated using the TrueDrop method, and each sample was measured three times and the average value was taken.

[0081] Method for characterizing membrane surface morphology: The surface morphology of the membrane was characterized by scanning electron microscopy (SEM, LEO1530vp, 5kV). Small pieces of graphene oxide / MOF composite membrane were cut out without violently squeezing the membrane surface and glued to the conductive adhesive. After gold treatment by ion sputtering for 45s, the membrane was observed under a scanning electron microscope with a measuring voltage of 3.0kV.

[0082] Membrane flux determination method: The flux of the prepared membrane is tested using a standard terminal filtration device equipped with a nitrogen bottle, a digital balance and a computer. The mass of the filtrate at different times is recorded by an electronic balance connected to a computer. The flux is calculated by the following formula:

[0083]

[0084] Where A is the effective membrane area (m 2 ), V is the permeate volume (L), t is the permeate time (h), and P is the transmembrane pressure (bar).

[0085] Membrane retention rate determination method: The retention performance of the membrane is measured by filtering a 5 ppm dye solution. Using the above flux measurement device, the dye concentration before and after filtration is measured by a UV-visible spectrophotometer. The retention rate is calculated by the following formula:

[0086]

[0087] Where R is the retention rate, C0 and C1 are the dye concentrations before and after filtration, respectively.

[0088] The pure water flux of the graphene oxide / MOF composite membrane prepared in Example 1 reached 1698.96 L·h -1 ·m -2 bar -1 ; At the same time, it was applied to the separation of common organic dyes such as Coomassie Brilliant Blue, Direct Red, Congo Red and Tiger Red Sodium Salt. The test analysis results obtained are as follows Figures 1 to 3 shown.

[0089] like Figure 1 As shown, the water contact angle of the graphene oxide / MOF composite film prepared in Example 1 is 7.2°, which has super hydrophilicity.

[0090] like Figure 2 As shown, the surface of the graphene oxide / MOF composite film prepared in Example 1 is dense and defect-free.

[0091] like Figure 3 As shown, the interception rate of the graphene oxide / MOF composite membrane prepared in Example 1 for the above-mentioned typical organic dyes is greater than 90%.

[0092] Example 2

[0093] (1) A 1.0 mg / mL graphene oxide solution was prepared, 25 μL of the graphene oxide solution was taken and diluted to 10 mL to obtain a 0.0025 mg / mL graphene oxide dispersion, and the graphene oxide dispersion was filtered using a nylon membrane to obtain a graphene oxide membrane.

[0094] (2) The graphene oxide film was immersed in a ZrCl4 solution (1.05 mol / L, 10 mL) for 16 h, and then taken out to obtain a zirconium ion / graphene oxide film.

[0095] (3) The remaining solution in step (2) was transferred to a 100 mL blue-capped bottle. L-aspartic acid (2.80 g, 21 mmol) was then added to the solution and stirred until completely dissolved to obtain a mixed solution.

[0096] (4) Then, the zirconium ion / graphene oxide film was immersed in the above mixed solution and reacted at 120° C. for 0.75 h. After the reaction was completed, the film was taken out and dried at room temperature of 25° C. for 20 h.

[0097] After the preparation is completed, the surface morphology of the graphene oxide / MOF composite membrane is characterized, such as Figure 4 As shown in Figure 2, the surface MOF grows more uniformly, and the pure water flux reaches 413.44 L·h -1 ·m -2 bar -1 .

[0098] Comparative Example 1

[0099] (1) A 1.0 mg / mL graphene oxide solution was prepared, 25 μL of the graphene oxide solution was taken and diluted to 10 mL to obtain a 0.0025 mg / mL graphene oxide dispersion, and the graphene oxide dispersion was filtered using a nylon membrane to obtain a graphene oxide membrane.

[0100] (2) The graphene oxide film was immersed in a ZrCl4 solution (0.95 mol / L, 10 mL) for 24 h, and then taken out to obtain a zirconium ion / graphene oxide film.

[0101] (3) The remaining solution in step (2) was transferred to a 100 mL blue-capped bottle. L-aspartic acid (2.80 g, 21 mmol) was then added to the solution and stirred until completely dissolved to obtain a mixed solution.

[0102] (4) Then, the zirconium ion / graphene oxide film was immersed in the above mixed solution and reacted at 120° C. for 0.25 h. After the reaction was completed, the film was taken out and dried at room temperature of 25° C. for 20 h.

[0103] After the preparation is completed, the structure of the composite membrane constructed by the above MOF and graphene oxide is characterized, such as Figure 5 As shown, compared with Example 1, the growth time is shorter, there are certain defects on the surface of the graphene oxide film, and the MOF grows less and is not dense enough.

[0104] Comparative Example 2

[0105] (1) A 1.0 mg / mL graphene oxide solution was prepared, 25 μL of the graphene oxide solution was taken and diluted to 10 mL to obtain a 0.0025 mg / mL graphene oxide dispersion, and the graphene oxide dispersion was filtered using a nylon membrane to obtain a graphene oxide membrane.

[0106] (2) The graphene oxide film was immersed in a ZrCl4 solution (0.95 mol / L, 10 mL) for 24 h, and then taken out to obtain a zirconium ion / graphene oxide film.

[0107] (3) The remaining solution in step (2) was transferred to a 100 mL blue-capped bottle. Then, (2.80 g, 21 mmol) of L-aspartic acid was added to the solution and stirred until completely dissolved to obtain a mixed solution.

[0108] (4) Then, the zirconium ion / graphene oxide film was immersed in the above mixed solution and reacted at 120° C. for 0.5 h. After the reaction was completed, the film was taken out and dried at room temperature of 25° C. for 20 h.

[0109] After the preparation is completed, the structure of the composite membrane constructed by the above MOF and graphene oxide is characterized, such as Figure 6 As shown, compared with Comparative Example 1, MOF grows more and grows on the surface of the graphene oxide film. It is connected with the graphene oxide, but not as dense as Example 1.

[0110] The composite membrane provided in the present invention combines the high specific surface area of ​​MOF materials with the excellent mechanical properties and chemical stability of graphene oxide materials, and shows good application prospects in the field of water treatment. The composite membrane can be used for intercepting and removing organic dyes in wastewater.

[0111] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A method for preparing a composite membrane based on a metal organic framework material, characterized in that: The following steps are involved: The graphene oxide dispersion is filtered onto the substrate membrane to obtain a graphene oxide membrane; Immersing the graphene oxide film in a zirconium ion-containing solution to obtain a zirconium ion / graphene oxide film; Immersing the zirconium ion / graphene oxide film in a precursor solution of a metal organic framework material and performing a heating reaction to obtain the composite film; Wherein, the precursor solution is a mixed solution containing an organic ligand and the zirconium ion-containing solution.

2. The method for preparing a composite film according to claim 1, characterized in that: The concentration of the zirconium ion solution is 0.95 mol / L to 1.05 mol / L; Preferably, the zirconium ion-containing solution comprises a zirconium chloride solution.

3. The method for preparing a composite film according to claim 1, characterized in that: The organic ligand is L-aspartic acid.

4. The method for preparing a composite film according to any one of claims 1 to 3, characterized in that: In the precursor solution, the mass ratio of the organic ligand to the zirconium ion-containing solution is 1:(0.8-1.2).

5. The method for preparing a composite film according to claim 1, characterized in that: The concentration of the graphene oxide dispersion is 0.001 mg / mL to 0.005 mg / mL, and the volume is 10 mL to 20 mL; Preferably, the graphene oxide film is immersed in the zirconium ion-containing solution for 16 hours to 24 hours.

6. The method for preparing a composite film according to claim 1, characterized in that: The temperature of the heating reaction is 118° C. to 122° C., and the time is 0.75 h to 1.25 h.

7. The method for preparing a composite film according to claim 1, characterized in that: The base film includes one of a cellulose acetate film, a nylon film, and a polytetrafluoroethylene film.

8. The method for preparing a composite film according to claim 1, characterized in that: The preparation method further comprises drying the prepared composite nanofiltration membrane; Preferably, the drying process is carried out at a temperature of 20°C to 30°C and for a time of 18h to 24h.

9. A composite membrane based on metal organic framework material, characterized in that: The composite film is prepared by the preparation method described in any one of claims 1 to 8.

10. Use of the metal organic framework material based composite membrane according to claim 9 or the metal organic framework material based composite membrane prepared by the preparation method according to any one of claims 1 to 8 in water purification.