Preparation method of desulfurization composite adsorbent and desulfurization composite adsorbent

By embedding active metal ions into alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier, and combining hydrothermal crystallization and impregnation methods to prepare desulfurization composite adsorbents, the problem of low COS removal rate in coke oven gas was solved, achieving efficient and low-cost desulfurization effect.

CN118892812APending Publication Date: 2024-11-05CIMC ENRIC ENGINEERING TECHNOLOGY CO LTD +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411294440.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing methods for removing COS from coke oven gas suffer from problems such as low desulfurization rate, harsh operating conditions, high energy consumption, and low safety of absorbents. Furthermore, the number and types of adsorption sites of conventional adsorbents are limited, resulting in low desulfurization performance.

Method used

A desulfurization composite adsorbent was prepared by a one-step hydrothermal crystallization method and a complete impregnation method. By embedding active metal ions into an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier, and combining the soft and hard acid-base theory, the sulfur capacity and specific surface area of ​​the adsorbent were increased. Activated carbon particles were used as a dispersion medium to promote the uniform dispersion of hydrotalcite particles on the surface of activated carbon.

Benefits of technology

The prepared desulfurization composite adsorbent has a large specific surface area, abundant active sites and high dispersibility, exhibiting good COS removal ability, mild operating conditions, low cost and significant environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892812A_ABST
    Figure CN118892812A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a desulfurization composite adsorbent and the desulfurization composite adsorbent. The preparation method of the desulfurization composite adsorbent comprises the following steps: weighing water-soluble magnesium salt, water-soluble aluminum salt and activated carbon powder, weighing sodium carbonate powder, and uniformly mixing the water-soluble magnesium salt, the water-soluble aluminum salt, the activated carbon powder and the sodium carbonate powder to obtain a mixture; uniformly dispersing the mixture in a sodium hydroxide solution to obtain a turbid liquid; crystallizing the turbid liquid; carrying out suction filtration on the crystallized turbid liquid to obtain a filter cake, washing the filter cake to be neutral by using deionized water, and then drying and grinding the filter cake to obtain an alkali modified activated carbon-magnesium aluminum hydrotalcite carrier; completely soaking the alkali modified activated carbon-magnesium aluminum hydrotalcite carrier in a metal salt solution, and dipping at room temperature for 2-4 hours; drying the impregnated solid particles to obtain solid particles; and roasting the solid particles in a protective atmosphere at 300-400 DEG C for 2 hours, and grinding to obtain the desulfurization composite adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adsorbents, and in particular to a preparation method of a desulfurization composite adsorbent and the desulfurization composite adsorbent. Background Art

[0002] Coke oven gas is a byproduct gas produced by high-temperature carbonization of coal. Its main components are H2 and CH4. It can be used not only to synthesize methanol, natural gas, prepare ammonia, hydrogen, etc., but also to heat coke ovens and city gas. It is a high-quality resource. However, the sulfides in coal will be converted into gaseous sulfides at high temperatures and enter the coke oven gas. These trace amounts of organic sulfur impurities restrict the use of coke oven gas in various industrial applications. Carbonyl sulfide (COS) is one of the main components of organic sulfur impurities in coke oven gas in my country. In the production process of chemical products, COS not only corrodes pipelines and equipment, but also causes poisoning and deactivation of various catalysts. In addition, COS emitted into the atmosphere will also produce sulfate aerosols by photolysis and oxidation, causing serious environmental pollution. In recent years, with the transformation of resources and the improvement of environmental protection requirements in my country, the issue of coke oven gas desulfurization has received widespread attention. Therefore, the removal of COS is of great significance to the application of coke oven gas in clean energy and the sustainable development of industry. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a desulfurization composite adsorbent and the desulfurization composite adsorbent to solve the problems in the prior art.

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a desulfurization composite adsorbent, comprising the following steps:

[0005] Weighing water-soluble magnesium salt, water-soluble aluminum salt and activated carbon powder respectively according to the mass percentage of magnesium: aluminum: activated carbon in the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier (0.15-0.17): (0.17-0.19): (0.23-0.26), weighing sodium carbonate powder according to the charge balance relationship between carbonate ions and magnesium ions and aluminum ions, and mixing the water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture;

[0006] The mixture is uniformly dispersed in a 1-10 mol / L sodium hydroxide solution to obtain a suspension;

[0007] Crystallizing the suspension at 60-90° C. for 2-4 hours;

[0008] The crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is dried at 100-110° C. for 4-6 hours and ground to obtain the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier;

[0009] The alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier is completely immersed in a metal salt solution and immersed at room temperature for 2 to 4 hours; wherein the metal ions in the metal salt solution include Cu 2+ 、Ni 2+ 、Zn 2+ 、Ag + Cr 3+ At least one of;

[0010] Drying the impregnated solid particles at 100-110° C. for 4-6 hours to obtain solid particles;

[0011] The solid particles are calcined at 300-400° C. for 2 hours under a protective atmosphere, and ground to obtain a desulfurization composite adsorbent, wherein the protective atmosphere includes at least one of nitrogen or an inert gas.

[0012] In one embodiment, the water-soluble magnesium salt includes at least one of magnesium chloride, magnesium sulfate and magnesium nitrate.

[0013] In one embodiment, the water-soluble aluminum salt includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate.

[0014] In one embodiment, the mixture is placed in the sodium hydroxide solution and ultrasonically dispersed at 10-30° C. for 30-60 min to obtain the suspension.

[0015] In one embodiment, the metal salt solution may be nitrate, acetate or chloride.

[0016] In one embodiment, the space velocity of the protective gas is 200 to 500 h -1 .

[0017] The present invention also provides a desulfurization composite adsorbent, which is prepared by the above-mentioned preparation method.

[0018] It can be seen from the above technical solution that the advantages and positive effects of the present invention are:

[0019] The preparation method of the present invention synthesizes the desulfurization composite adsorbent by a one-step hydrothermal crystallization method and a complete impregnation method. Active metal ions in alkali-modified activated carbon and metal salt solution are embedded in the interlayer of magnesium-aluminum hydrotalcite to obtain a desulfurization composite adsorbent with abundant active sites. Active metal ions are loaded on alkali-modified activated carbon / magnesium-aluminum hydrotalcite by an impregnation method, and the sulfur capacity of the desulfurization composite adsorbent is increased by combining the soft and hard acid-base theory with COS. Activated carbon particles are used as a dispersion medium to increase the specific surface area of ​​the desulfurization composite adsorbent, promote the in-situ growth and uniform dispersion of hydrotalcite particles on the surface of activated carbon particles, and the layered structure based on hydrotalcite helps the activated carbon to form a stable pore environment. Therefore, the desulfurization composite adsorbent prepared by the present invention has the characteristics of large specific surface area, abundant active sites, and high dispersion, and exhibits good desulfurization ability.

[0020] The preparation method of the present invention is operated under normal pressure, which greatly reduces technical requirements, saves operating costs, and has high economic, environmental and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the process of the desulfurization composite adsorbent in the present invention.

[0022] Figure 2 It is the dynamic penetration curve of Example 1 and the comparative example. DETAILED DESCRIPTION

[0023] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions and illustrations therein are essentially used for illustration purposes rather than for limiting the present invention.

[0024] In order to further illustrate the principle and structure of the present invention, preferred embodiments of the present invention are now described in detail with reference to the accompanying drawings.

[0025] At present, the main methods for removing COS include high-temperature hydrogenation, hydrolysis, absorption and adsorption. Among them, the high-temperature hydrogenation method is to convert COS into H2S under high temperature conditions of 300℃ to 500℃ and then remove it with an adsorbent. However, the operating conditions of the high-temperature hydrogenation method are harsh and the process energy consumption is high. The hydrolysis method is to hydrolyze COS into H2S and CO2 using a catalyst in the presence of water vapor and then remove it. The process route of the hydrolysis method is cumbersome. The absorption method mainly uses organic amine solvents to absorb COS, but organic amines are highly toxic, low in safety and have a low absorption rate.

[0026] Since COS is a linear molecule with a stable structure, the above three methods all have the problem of low desulfurization rate.

[0027] The adsorption method has the advantages of mild conditions, simple operation, fast desulfurization speed, low energy consumption, easy regeneration of adsorbent, and no by-products during the desulfurization process. In addition, this method is not limited by reaction thermodynamics, so it is particularly suitable for deep removal of low-concentration COS.

[0028] The key to adsorption desulfurization is the adsorbent used, and its desulfurization rate mainly depends on the structural characteristics of the material, such as specific surface area and pore size, as well as adsorption activity, including the number and type of active sites. At present, common adsorption materials include activated carbon, metal oxides, metal hydroxides, etc. Among them, activated carbon is cheap and easy to obtain, has a stable structure, and has a large specific surface area and a variety of pore structures. It is widely used in the treatment of industrial waste gas. However, the removal mechanism of activated carbon for COS is mainly physical adsorption, so the desulfurization rate is low. Subsequently, a large number of hydroxyl groups can be introduced on the surface of activated carbon through alkali modification, thereby improving the desulfurization rate of activated carbon, but the increase in adsorption sulfur capacity is limited. Metal oxide desulfurizers mainly include Cu2O, ZnO, Ni2O, Cr2O3, etc. It mainly forms σ and π bonds with COS through chemical forces, and has the characteristics of high selectivity and high desulfurization rate. However, due to the low specific surface area of ​​metal oxides, the overall adsorption sulfur capacity is not large. Among metal hydroxides, hydrotalcite is a layered double hydroxide (LDHs). It has become a highly regarded desulfurization composite adsorbent due to its excellent ion exchangeability and unique adjustable layered structure. 2+ , Al-O, hydroxyl and other desulfurization active sites, and has good adsorption and removal performance for COS. However, the accumulation of hydrotalcite sheets and the collapse of the interlayer structure cause the decrease of adsorption performance.

[0029] In summary, although conventional adsorbents can remove a certain amount of COS, their overall desulfurization performance is not high due to the single type of adsorption sites and the limited number of adsorption sites. Therefore, the present invention provides a method for preparing a desulfurization composite adsorbent having a large number of adsorption sites and high desulfurization performance, and a desulfurization composite adsorbent.

[0030] Figure 1 A schematic diagram of the process for preparing a desulfurization composite adsorbent is shown in FIG. Figure 1 The preparation method of the desulfurization composite adsorbent comprises the following steps:

[0031] S1. According to the mass percentage of magnesium: aluminum: activated carbon in the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier (0.15-0.17): (0.17-0.19): (0.23-0.26), water-soluble magnesium salt, water-soluble aluminum salt and activated carbon powder are weighed respectively, and sodium carbonate powder is weighed according to the charge balance relationship between carbonate ions and magnesium ions and aluminum ions, and the water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder are mixed uniformly to obtain a mixture.

[0032] Specifically, the water-soluble magnesium salt includes at least one of magnesium chloride, magnesium sulfate and magnesium nitrate.

[0033] The water-soluble aluminum salt includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate.

[0034] The mass percentage of magnesium:aluminum:activated carbon in the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier is preferably (0.15-0.17):(0.17-0.19):(0.23-0.26).

[0035] S2. The mixture is uniformly dispersed in a 1-10 mol / L sodium hydroxide solution to obtain a suspension.

[0036] Specifically, the mixture is placed in a sodium hydroxide solution and ultrasonically dispersed at 10 to 30° C. for 30 to 60 minutes to obtain a suspension.

[0037] S3. Crystallize the suspension at 60-90°C for 2-4h.

[0038] The suspension can be transferred to a reaction vessel and subjected to a crystallization reaction at 60 to 90° C. under normal pressure for 2 to 4 hours.

[0039] The suspension can also be transferred to a water bath for crystallization reaction.

[0040] S4. The crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is dried at 100-110° C. for 4-6 hours and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0041] S5, completely immersing the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in a metal salt solution at room temperature for 2 to 4 hours; wherein the metal ions in the metal salt solution include Cu 2+ 、Ni 2+ 、Zn 2+ 、Ag + Cr 3+ At least one of .

[0042] The metal ion of the metal salt solution is Cu 2+ When the desulfurization composite adsorbent is used, the active component is cuprous oxide (Cu2O).

[0043] The metal ion of the metal salt solution is Ni 2+ When the desulfurization composite adsorbent is used, the active component is nickel oxide (Ni2O).

[0044] The metal ion of the metal salt solution is Zn 2+ When the desulfurization composite adsorbent is used, the active component is zinc oxide (ZnO).

[0045] The metal ion of the metal salt solution is Ag + When the desulfurization composite adsorbent is used, the active component is silver oxide (AgO).

[0046] The metal ion of the metal salt solution is Cr 3+ When the desulfurization composite adsorbent is used, the active component is chromium oxide (Cr2O3).

[0047] Specifically, the metal salt solution is added dropwise onto the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier, so that the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier is completely immersed in the metal salt solution.

[0048] The metal ions in the metal salt solution are active ingredients. The metal ions are loaded on the alkali-modified activated carbon / magnesium-aluminum hydrotalcite through the impregnation method, and combined with COS through the soft and hard acid-base theory to increase the sulfur capacity of the desulfurization composite adsorbent.

[0049] Specifically, the metal salt solution alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier can be nitrate, acetate or chloride. Preferably, the metal salt solution can be nitrate or chloride.

[0050] The alkali-modified activated carbon-magnesium aluminum hydrotalcite support is completely immersed in the metal salt solution, that is, the complete impregnation method (also called the equal volume impregnation method), to ensure that the pore volume of the alkali-modified activated carbon-magnesium aluminum hydrotalcite support can be 100% occupied by the metal salt solution.

[0051] S6. Dry the impregnated solid particles at 100-110° C. for 4-6 hours to obtain solid particles.

[0052] S7. The solid particles are calcined at 300-400° C. for 2 h under a protective atmosphere, and ground to obtain a desulfurization composite adsorbent, wherein the protective atmosphere includes at least one of nitrogen or an inert gas.

[0053] Specifically, the space velocity of the protective gas is 200 to 500 h -1 .

[0054] The preparation method of the present application uses water-soluble magnesium salt, water-soluble aluminum salt, and sodium carbonate powder as raw materials for preparing magnesium aluminum hydrotalcite, and activated carbon particles as dispersant raw materials, and adds sodium hydroxide solution, and adopts a one-step hydrothermal crystallization method under normal pressure to prepare an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier. Then, the active component salt solution is slowly dripped onto the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier by a complete impregnation method, and after drying and roasting, a desulfurization composite adsorbent is obtained. That is, the desulfurization composite adsorbent is synthesized by a one-step hydrothermal crystallization method and a complete impregnation method.

[0055] The present invention embeds the active metal ions in the alkali-modified activated carbon and the metal salt solution into the interlayer of the magnesium-aluminum hydrotalcite to obtain a desulfurization composite adsorbent with abundant active sites. The active sites include the physical adsorption sites of the activated carbon, the hydroxyl active sites of the alkali-modified activated carbon, the Mg of the magnesium-aluminum hydrotalcite, and the Mg of the magnesium-aluminum hydrotalcite. 2+ , Al-O, Cu2O and Al-OH. Active metal ions are loaded on alkali-modified activated carbon / magnesium-aluminum hydrotalcite by impregnation, and the sulfur capacity of the desulfurization composite adsorbent is increased by combining with COS through the soft-hard acid-base theory. Activated carbon particles are used as dispersion medium to increase the specific surface area of ​​the desulfurization composite adsorbent, promote the in-situ growth and uniform dispersion of hydrotalcite particles on the surface of activated carbon particles, and the layered structure of hydrotalcite helps the activated carbon to form a stable pore environment. Therefore, the desulfurization composite adsorbent prepared by the present invention has the characteristics of large specific surface area, rich active sites, high dispersion, and exhibits good desulfurization ability.

[0056] The preparation method of the present application is operated under normal pressure, which greatly reduces technical requirements, saves operating costs, and has high economic, environmental and social benefits.

[0057] The present application also provides a desulfurization composite adsorbent, which is prepared using the above-mentioned preparation method.

[0058] The inventors of the present application have achieved the preparation of a desulfurization composite adsorbent by strictly designing the content of each component and the parameters in each step. The method is introduced below through various examples.

[0059] Example 1

[0060] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0061] S11, weighing 1.29 g of magnesium chloride hexahydrate, 1.54 g of aluminum chloride hexahydrate and 0.23 g of activated carbon powder, weighing 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mixing the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0062] S12. The mixture was uniformly dispersed in 20 mL of 1 mol / L sodium hydroxide solution to obtain a suspension.

[0063] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 10° C. for 60 min to obtain a suspension.

[0064] S13, crystallizing the suspension at 60°C for 4h.

[0065] S14, filtering the crystallized suspension to obtain a filter cake, washing the filter cake with deionized water until it is neutral, and then drying the filter cake in an oven at 100° C. for 6 hours, and grinding to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0066] S15. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the copper nitrate solution and immerse it at room temperature for 2 hours.

[0067] S16, drying the impregnated solid particles at 100° C. for 6 hours to obtain solid particles.

[0068] S17. The solid particles are calcined at 300° C. for 2 h under a nitrogen atmosphere and ground to obtain a desulfurization composite adsorbent.

[0069] Among them, the nitrogen space velocity is 200h -1 .

[0070] Example 2

[0071] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0072] S21. Weigh 0.74 g of magnesium sulfate, 1.08 g of aluminum sulfate and 0.26 g of activated carbon powder, weigh 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mix the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0073] S22. The mixture is uniformly dispersed in 10 mL of 5 mol / L sodium hydroxide solution to obtain a suspension.

[0074] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 30° C. for 30 min to obtain a suspension.

[0075] S23. Crystallize the suspension at 90° C. for 2 h.

[0076] S24, the crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is placed in an oven at 110° C. and dried for 4 hours, and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0077] S25. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the zinc nitrate solution and immerse it at room temperature for 4 hours.

[0078] S26, drying the impregnated solid particles at 110° C. for 4 hours to obtain solid particles.

[0079] S27. The solid particles are calcined at 400° C. for 2 h under a nitrogen atmosphere and ground to obtain a desulfurization composite adsorbent.

[0080] Among them, the nitrogen space velocity is 500h -1 .

[0081] Example 3

[0082] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0083] S31. Weigh 0.92 g of magnesium nitrate, 1.5 g of aluminum nitrate and 0.23 g of activated carbon powder, weigh 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mix the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0084] S32. Disperse the mixture evenly in 20 mL of 10 mol / L sodium hydroxide solution to obtain a suspension.

[0085] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 20° C. for 40 min to obtain a suspension.

[0086] S33, crystallizing the suspension at 80°C for 3h.

[0087] S34, the crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is placed in an oven at 105° C. and dried for 5 hours, and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0088] S35. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the nickel nitrate solution and immerse it at room temperature for 3 hours.

[0089] S36, drying the impregnated solid particles at 105° C. for 5 h to obtain solid particles.

[0090] S37. The solid particles are calcined at 350° C. for 2 h in a helium atmosphere and ground to obtain a desulfurization composite adsorbent.

[0091] Among them, the nitrogen space velocity is 300h -1 .

[0092] Example 4

[0093] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0094] S41. Weigh 0.98 g of magnesium nitrate, 1.21 g of aluminum sulfate and 0.25 g of activated carbon powder, weigh 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mix the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0095] S42. Disperse the mixture evenly in 15 mL of 2 mol / L sodium hydroxide solution to obtain a suspension.

[0096] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 15° C. for 50 min to obtain a suspension.

[0097] S43. Crystallize the suspension at 75°C for 2.5h.

[0098] S44, the crystallized suspension was filtered to obtain a filter cake, the filter cake was washed with deionized water until it was neutral, and then the filter cake was placed in an oven at 108° C. for 4.5 hours and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0099] S45. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the silver nitrate solution and immerse it at room temperature for 3.5 hours.

[0100] S46, drying the impregnated solid particles at 102° C. for 5.5 h to obtain solid particles.

[0101] S47. The solid particles are calcined at 360° C. for 2 h in a helium atmosphere and ground to obtain a desulfurization composite adsorbent.

[0102] Among them, the nitrogen space velocity is 450h -1 .

[0103] Example 5

[0104] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0105] S51. Weigh 1.04 g of magnesium nitrate, 1.14 g of aluminum sulfate and 0.24 g of activated carbon powder, weigh 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mix the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0106] S52. Disperse the mixture uniformly in 16 mL of 4 mol / L sodium hydroxide solution to obtain a suspension.

[0107] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 25° C. for 30 min to obtain a suspension.

[0108] S53, crystallizing the suspension at 85°C for 3.5h.

[0109] S54, the crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is placed in an oven at 100° C. for 5 hours and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0110] S55. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the chromium nitrate solution and immerse it at room temperature for 2.5 hours.

[0111] S56, drying the impregnated solid particles at 106° C. for 5 hours to obtain solid particles.

[0112] S57. The solid particles are calcined at 380° C. for 2 h in a helium atmosphere and ground to obtain a desulfurization composite adsorbent.

[0113] Among them, the nitrogen space velocity is 350h -1 .

[0114] Example 6

[0115] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0116] S61. Weigh 1.04 g of magnesium nitrate, 1.42 g of aluminum nitrate and 0.26 g of activated carbon powder, weigh 1.77 g of sodium carbonate powder according to the charge balance relationship between carbonate ions, magnesium ions and aluminum ions, and mix the above water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture.

[0117] S62. Disperse the mixture evenly in 20 mL of 6 mol / L sodium hydroxide solution to obtain a suspension.

[0118] The mixture was placed in a sodium hydroxide solution and ultrasonically dispersed at 20° C. for 50 min to obtain a suspension.

[0119] S63. Crystallize the suspension at 70°C for 3h.

[0120] S64. The crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is placed in an oven at 105° C. and dried for 4 hours, and ground to obtain an alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier.

[0121] S65. Completely immerse the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier in the zinc chloride solution and immerse it at room temperature for 3 hours.

[0122] S66. Dry the impregnated solid particles at 10° C. for 5 h to obtain solid particles.

[0123] S67. The solid particles are calcined at 350° C. for 2 h in a helium atmosphere and ground to obtain a desulfurization composite adsorbent.

[0124] Among them, the space velocity of nitrogen is 360h -1 .

[0125] Comparative Example 1

[0126] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0127] S71. Mix 1.43 g of magnesium chloride hexahydrate and 1.70 g of aluminum chloride hexahydrate and add them into deionized water, which is recorded as solution A.

[0128] S72. Add deionized water to 1.77 g of sodium carbonate and 2 g of sodium hydroxide, and record it as solution B.

[0129] S73. Add solutions A and B dropwise into beaker C at a constant speed, adjust the pH to about 10, seal and stir with magnetic force for 30 minutes, put into a water bath at 80°C for 3 hours, cool, filter, rinse the filter cake with deionized water until the pH of the washing solution is close to 7, dry and grind to obtain magnesium aluminum hydrotalcite.

[0130] S74. Add 0.23 g of activated carbon into a beaker, add 20 mL of 5 mol / L sodium hydroxide solution into the beaker, seal, ultrasonically disperse for 30 minutes, filter and dry to obtain alkali-modified activated carbon.

[0131] S75. Using an impregnation method, alkali-modified activated carbon and magnesium-aluminum hydrotalcite are mixed, deionized water is added, and ultrasonic vibration is performed for 30 minutes. The filter cake is filtered, dried, and ground to obtain an alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier.

[0132] S76. Slowly drop 5 mL of a solution containing 0.24 g of copper nitrate trihydrate onto 1.25 g of the above support and soak at room temperature for 3 hours.

[0133] S77, drying the sample in an oven at 105° C. for 4 h, and calcining the sample at 350° C. in a nitrogen atmosphere for 2 h. After calcination, grinding the obtained product, and finally obtaining a desulfurization composite adsorbent loaded with 10% (mass fraction) of active components.

[0134] Comparative Example 2

[0135] The preparation method of the desulfurization composite adsorbent in this embodiment comprises the following steps:

[0136] S81. 1.43 g of magnesium chloride hexahydrate, 1.70 g of aluminum chloride hexahydrate and 0.26 g of activated carbon were mixed and added into deionized water, and ultrasonicated for 5 min. This was recorded as solution A.

[0137] S82. Add deionized water to 1.77 g of sodium carbonate and 2 g of sodium hydroxide, and record it as solution B.

[0138] S83. Add solutions A and B dropwise into beaker C at a constant speed, adjust the pH to about 10, seal and stir with magnetic force for 30 minutes, place in a water bath at 80°C for 3 hours, cool, filter, rinse the filter cake with deionized water until the pH of the washing solution is close to 7, dry and grind to obtain magnesium aluminum hydrotalcite.

[0139] S84. Add 0.26 g of activated carbon and magnesium aluminum hydrotalcite into a beaker, add deionized water, perform ultrasonic vibration for 30 minutes, filter the obtained filter cake, dry and grind it to obtain an activated carbon-magnesium aluminum hydrotalcite carrier.

[0140] S85. Slowly drop 5 mL of a solution containing 0.24 g of copper nitrate trihydrate onto 1.25 g of the above-mentioned activated carbon-magnesium aluminum hydrotalcite carrier and soak at room temperature for 3 hours.

[0141] S86, drying the sample in an oven at 105° C. for 4 h, and calcining the sample in a nitrogen atmosphere at 350° C. for 2 h. After calcination, grinding the obtained product, and finally obtaining a desulfurization composite adsorbent loaded with 10% (mass fraction) of active components.

[0142] The performance of the desulfurization composite adsorbent prepared in Example 1 and Comparative Examples 1-2 was evaluated respectively, and the evaluation method was as follows:

[0143] The simulated coke oven gas components are prepared from standard cylinder gases, including high-purity CH4, CO, H2 and standard COS gas (99.0% H2 + 1.0% COS, percentage is volume fraction), and the nitrogen volume space velocity is preferably 300h -1 , which is accurately controlled by a mass flow meter. The COS mass concentration (in S) is 666.6 mg / m 3 . Weigh 0.25g of desulfurizer and load it into a U-shaped reaction tube. Before the desulfurization performance evaluation experiment begins, N2 is introduced to purge the desulfurizer for 1 hour, and then N2 is switched to simulated coke oven gas. The desulfurizer and the raw gas are fully in contact in the reaction tube, and the COS concentration of the outlet gas is regularly detected by a gas chromatograph (the detector is FPD). When the COS concentration in the outlet gas reaches 10% of the COS in the simulated coke oven gas, it is considered that the adsorbent has penetrated, and the experiment is stopped at this time. Afterwards, the breakthrough sulfur capacity of the adsorbent is calculated based on the reaction time (breakthrough time) when the adsorbent penetrates.

[0144] Table 1 Performance of desulfurization composite adsorbent

[0145] Examples and Comparative Examples Breakthrough time (min) Penetration sulfur capacity g / mg Example 1 509 20.38 Example 2 353.4 14.13 Example 3 260.7 10.43 Example 4 340 13.6 Example 5 422.9 16.91 Example 6 348.6 13.94 Comparative Example 1 504 20.16 Comparative Example 2 381.8 15.27

[0146] It can be seen from Table 1 that the breakthrough time and breakthrough sulfur capacity of the desulfurization composite adsorbent of Example 1 are the same as those of Comparative Example 1, that is, the one-step method of the present application can achieve the desulfurization effect of the two-step method in the prior art.

[0147] Combination Figure 2 It can be seen that the penetration time and penetration sulfur capacity of the desulfurization composite adsorbent of Example 1 are significantly better than those of Comparative Example 2. Therefore, whether the activated carbon is alkali-modified has a greater impact on the COS adsorption performance. The reason is: although activated carbon has a high specific surface area and a microporous structure, the material mainly relies on the surface and pores for physical adsorption. The kinetic diameter of COS is about 3 to 9A, and it is sometimes excluded from the micropores of activated carbon, resulting in low adsorption capacity of unmodified activated carbon. The alkali modification process expands the micropores of the activated carbon and forms many pores of different sizes. In addition, alkali modification can also increase the alkali active sites (-OH) on the surface of activated carbon, which is also an important functional group for removing COS. Based on this, the alkali-modified activated carbon significantly improves its adsorption capacity for COS.

[0148] Although the present invention has been described with reference to several typical embodiments, it should be understood that the terms used are illustrative and exemplary, rather than restrictive. Since the present invention can be embodied in a variety of forms without departing from the spirit or essence of the invention, it should be understood that the above embodiments are not limited to any of the foregoing details, but should be interpreted broadly within the spirit and scope defined by the appended claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the appended claims.

Claims

1. A method for preparing a desulfurization composite adsorbent, characterized in that: The following steps are involved: Weighing water-soluble magnesium salt, water-soluble aluminum salt and activated carbon powder respectively according to the mass percentage of magnesium: aluminum: activated carbon in the alkali-modified activated carbon-magnesium-aluminum hydrotalcite carrier (0.15-0.17): (0.17-0.19): (0.23-0.26), weighing sodium carbonate powder according to the charge balance relationship between carbonate ions and magnesium ions and aluminum ions, and mixing the water-soluble magnesium salt, water-soluble aluminum salt, activated carbon powder and sodium carbonate powder to obtain a mixture; The mixture is uniformly dispersed in a 1-10 mol / L sodium hydroxide solution to obtain a suspension; Crystallizing the suspension at 60-90° C. for 2-4 hours; The crystallized suspension is filtered to obtain a filter cake, the filter cake is washed with deionized water until it is neutral, and then the filter cake is dried at 100-110° C. for 4-6 hours and ground to obtain the alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier; The alkali-modified activated carbon-magnesium aluminum hydrotalcite carrier is completely immersed in a metal salt solution and immersed at room temperature for 2 to 4 hours; wherein the metal ions in the metal salt solution include Cu 2+ 、Ni 2+ 、Zn 2+ 、Ag + Cr 3+ At least one of; Drying the impregnated solid particles at 100-110° C. for 4-6 hours to obtain solid particles; The solid particles are calcined at 300-400° C. for 2 hours under a protective atmosphere, and ground to obtain a desulfurization composite adsorbent, wherein the protective atmosphere includes at least one of nitrogen or an inert gas.

2. The method for preparing the desulfurization composite adsorbent according to claim 1, characterized in that: The water-soluble magnesium salt includes at least one of magnesium chloride, magnesium sulfate and magnesium nitrate.

3. The method for preparing the desulfurization composite adsorbent according to claim 1, characterized in that: The water-soluble aluminum salt includes at least one of aluminum chloride, aluminum sulfate and aluminum nitrate.

4. The method for preparing the desulfurization composite adsorbent according to claim 1, characterized in that: The mixture is placed in the sodium hydroxide solution and ultrasonically dispersed at 10-30° C. for 30-60 min to obtain the suspension.

5. The method for preparing the desulfurization composite adsorbent according to claim 1, characterized in that: The metal salt solution may be nitrate, acetate or chloride.

6. The method for preparing the desulfurization composite adsorbent according to claim 1, characterized in that: The space velocity of the protective gas is 200 to 500 h -1 .

7. A desulfurization composite adsorbent, characterized in that: The method is described in any one of claims 1 to 6.

Citation Information

Patent Citations

  • Catalyst for hydrolyzing carbonyl sulfur and preparation method thereof

    CN101559379A

  • Preparation method of load-type desulfurizer

    CN101590395A

  • Carbon-based catalyst for desulfurization and denitrification as well as preparation method and application of catalyst

    CN104368323A

  • Adsorption desulfurization additive, as well as preparation method and desulfurization system thereof

    CN104549131A

  • Preparation method of hydrotalcite-like catalyst used for removing of HCN and COS gas

    CN107626295A