Preparation method of TNT / TCPP material for printing and dyeing wastewater treatment, TNT / TCPP material and application of TNT / TCPP material
Titanate nanotubes were prepared by hydrothermal method and combined with TCPP to form TNT/TCPP materials, which solved the shortcomings of traditional TiO2 photocatalytic materials in environmental pollution treatment, significantly improved photocatalytic and electrochemical properties, and achieved efficient Printing and dyeing wastewater treatment.
Patent Information
- Application Number
- CN202410938715.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-14
- Publication Date
- 2024-11-05
AI Technical Summary
In the environmental pollution treatment of traditional TiO2 photocatalytic materials, there are problems such as photogenerated carriers that are prone to recombination, affecting reaction activity, insufficient photocatalytic effect of printing and dyeing wastewater and poor electrochemical performance.
Titanate nanotubes (TNTs) are prepared by hydrothermal method, and TNT/TCPP materials are combined in different proportions with TCPP. Through stirring and ultrasonic treatment technology, the physical and chemical properties of the materials are optimized and the photocatalytic degradation capabilities are improved.
The effect of photocatalytic degradation of dyes is improved, the photogenerated carrier separation efficiency is optimized, the ultraviolet-visible absorption and electrochemical properties are improved, and the ability to treat printing and dyeing wastewater is significantly improved.
Smart Images

Figure CN118892820A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental material preparation, and in particular to a TNT / TCPP material preparation method for printing and dyeing wastewater treatment, a TNT / TCPP material and an application thereof. Background Art
[0002] In recent years, photocatalytic degradation has become an important method for environmental pollution treatment, that is, photocatalytic materials can effectively decompose organic pollutants and kill bacteria under the irradiation of light sources. Among the many photocatalyst materials, TiO 2 Because of its non-toxicity, strong oxidation ability, high catalytic efficiency, and zero pollution emission after treatment, it has been increasingly used. Under ultraviolet light, TiO 2 Hydroxyl radicals and superoxide anions can be produced through electron transition to degrade organic matter.
[0003] The current traditional TiO 2 Photocatalytic materials still have many shortcomings in environmental pollution treatment, such as: photogenerated carriers are very easy to recombine, reaction activity is affected, the photocatalytic effect on printing and dyeing wastewater needs to be improved, and the electrochemical performance is poor. Summary of the invention
[0004] The present invention provides a method for preparing a TNT / TCPP material for treating printing and dyeing wastewater, a TNT / TCPP material and application thereof, aiming to solve the above-mentioned problems existing in the background technology.
[0005] The technical solution provided by the present invention is as follows:
[0006] The first aspect of the present invention provides a method for preparing a TNT / TCPP material for treating printing and dyeing wastewater, comprising the following steps:
[0007] Step S1: Mix NaOH solution with P-25 type TiO 2 The powders are mixed, stirred evenly, and then subjected to hydrothermal treatment to obtain a first reaction product;
[0008] Step S2, transferring the first reaction product into deionized water, stirring and dispersing it uniformly, and then centrifuging it to remove the supernatant, and repeatedly washing and centrifuging the precipitate until the pH value of the washing liquid reaches 7.0;
[0009] Step S3, adding the first reaction product whose washing liquid is neutral after water washing into a dilute hydrochloric acid solution for pickling, and after the pickling is completed, washing again with deionized water until the pH value is 7.0;
[0010] Step S4, drying the first reaction product after washing again, and grinding it sufficiently after drying to obtain TiO 2Nanotube powder samples;
[0011] Step S5: 2 The nanotube powder sample was placed in anhydrous ethanol and subjected to ultrasonic treatment to make the TiO 2 The nanotube powder samples were uniformly dispersed in anhydrous ethanol;
[0012] Step S6: uniformly disperse the TiO 2 The mixed solution of the nanotube powder sample is added to a uniformly dispersed TCPP ethanol solution, stirred under heating conditions until the ethanol is completely evaporated, and then dried to obtain the TNT / TCPP material.
[0013] Further, in step S1, the concentration of the NaOH solution is 10 mol / L;
[0014] The NaOH solution was mixed with P-25 type TiO 2 The specific powder mixing is as follows: 0.8 g of P-25 type TiO 2 The powder is mixed with 50.0 ml of the NaOH solution having a concentration of 10 mol / L;
[0015] The temperature of the hydrothermal treatment is 150° C. and the time is 48 hours.
[0016] Furthermore, in step S3, the concentration of the dilute hydrochloric acid solution is 0.1 mol / L, and the volume of the added dilute hydrochloric acid is 200 ml.
[0017] Furthermore, in step S4, the drying is performed in an oven at a constant temperature of 70°C.
[0018] Further, in step S5, the TiO 2 The nanotube powder sample was placed in anhydrous ethanol and ultrasonically treated as follows:
[0019] Take 300 mg of the TiO 2 The nanotube powder sample was placed in 40 mL of anhydrous ethanol and sonicated for 30 minutes using ultrasound.
[0020] Further, in step S6, the TCPP and the TiO 2 The mass ratio of nanotube powder samples is 0.1%-1%;
[0021] The stirring is carried out by using a magnetic stirrer at a temperature of 80°C;
[0022] The drying treatment is specifically performed by heating in an oven at 80° C. for 10 hours.
[0023] Furthermore, in step S1, the NaOH solution is mixed with P-25 type TiO 2 The powders are mixed, stirred evenly and then subjected to hydrothermal treatment to obtain a first reaction product, comprising the following steps:
[0024] 20.0 g of NaOH was weighed using an electronic balance, and then dissolved in 50.0 ml of deionized water to prepare a NaOH solution with a concentration of 10 mol / L under magnetic stirring;
[0025] Weigh 0.8 g of P-25 TiO 2 powder, and mixed it with 50.0 ml of NaOH solution in a Teflon-lined reactor and stirred magnetically for 30 min;
[0026] The magnetic stirrer was removed, the reactor was sealed, and the polytetrafluoroethylene liner of the reactor was placed in a stainless steel autoclave. The lid was tightened, and the stainless steel autoclave was placed in an oven for hydrothermal treatment at 150° C. for 48 hours to obtain the first reaction product.
[0027] Further, in step S2, the first reaction product is transferred to deionized water, stirred and dispersed uniformly, and then centrifuged to remove the supernatant, and the precipitate is repeatedly washed with water and centrifuged until the pH value of the washing liquid reaches 7.0, specifically:
[0028] After the stainless steel high-pressure reactor is naturally cooled to room temperature, the first reaction product is taken out and transferred to deionized water, and a suspension is obtained after being stirred and dispersed evenly. The suspension is transferred to a centrifuge tube, 80.0 ml of the suspension is added to each tube, and the centrifuge tube is placed in a centrifuge for centrifugal separation, the supernatant is removed, and this process is repeated until the pH value of the washing liquid reaches 7.0.
[0029] A second aspect of the present invention provides a TNT / TCPP material, which is prepared by the above-mentioned method for preparing the TNT / TCPP material for treating printing and dyeing wastewater.
[0030] A third aspect of the present invention is an application of the above TNT / TCPP material in environmental pollution treatment.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The invention provides a method for preparing a TNT / TCPP material for treating printing and dyeing wastewater, a TNT / TCPP material and an application thereof. Titanate nanotubes are prepared by a hydrothermal method, and then the prepared TNT and TCPP are used to prepare the TNT / TCPP material in different ratios. Characterization experiments of TNT and TNT / TCPP materials are performed by X-ray diffraction analysis (XRD) to determine the physical and chemical properties of the materials. Then, the prepared material is used to perform a photocatalytic dye degradation experiment. By extracting samples of different illumination times, the photocatalytic sample degradation performance test is performed. The results show that the TNT / TCPP material prepared by the invention has a better photocatalytic dye degradation effect, and compared with the traditional TiO 2 Photocatalytic materials, TNT / TCPP materials are optimized in terms of photogenerated carrier separation efficiency, photocatalytic performance is improved, have better UV-visible absorption performance, and electrochemical performance is improved. The 1.0% TNT / TCPP material prepared by the present invention has high efficiency in treating printing and dyeing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a SEM image of the TNT material in the embodiment of the present invention;
[0034] Figure 2 This is a SEM image of the TNT / TCPP material prepared in the embodiment of the present invention;
[0035] Figure 3 TEM image of TNT material in an embodiment of the present invention;
[0036] Figure 4 TEM image of the TNT / TCPP material prepared in the embodiment of the present invention;
[0037] Figure 5 TEM image of 1.0% TNT / TCPP material prepared in an embodiment of the present invention;
[0038] Figure 6 This is a TEM analysis diagram of 1.0% TNT / TCPP material in an embodiment of the present invention;
[0039] Figure 7 The X-ray diffraction analysis diagram of P-25, TNT and TNT / TCPP materials in the embodiments of the present invention;
[0040] Figure 8 The infrared transmission spectra of P-25, TNT and TNT / TCPP materials in the embodiments of the present invention;
[0041] Fig. 9 It is the infrared transmission spectrum of the TCPP material in the embodiment of the present invention;
[0042] Fig.10The XPS spectra of P-25 and 1.0% TNT / TCPP materials in the examples of the present invention;
[0043] Fig.11 Schematic diagram of UV-visible absorption spectra of P-25, TCPP, TNT and TNT / TCPP materials in the embodiments of the present invention;
[0044] Fig.12 The semiconductor band gap spectra of P-25 and TCPP in the embodiments of the present invention;
[0045] Fig.13 The band gap spectrum of TNT and TNT / TCPP materials in the embodiments of the present invention;
[0046] Fig.14 The fluorescence intensity characterization spectrum of TNT and 1.0% TNT / TCPP materials in the embodiment of the present invention;
[0047] Fig.15 The electrochemical TPC spectra of TNT and 1.5% TNT / TCPP in the embodiment of the present invention;
[0048] Fig.16 The photocatalytic dark reaction effect diagram of TNT and different TNT / TCPP materials in the embodiment of the present invention;
[0049] Fig.17 The photocatalytic photoreaction effect diagram of TNT and different TNT / TCPP materials in the embodiment of the present invention;
[0050] Fig.18 The photocatalytic degradation rate effect diagram of TNT and different TNT / TCPP materials in the embodiment of the present invention;
[0051] Fig.19 It is a bar graph of the degradation rate of TNT and different TNT / TCPP materials in the embodiment of the present invention;
[0052] Fig. 20 This is the superoxide spectrum of the 1.0% TNT / TCPP material in the embodiment of the present invention;
[0053] Fig.21 This is the EPR hydroxyl spectrum of the 1.0% TNT / TCPP material in the embodiment of the present invention;
[0054] Fig. 22 This is a spectrum of the holes in the 1.0% TNT / TCPP material in the example of the present invention. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Therefore, the detailed description of the embodiments of the present application provided below in conjunction with the drawings is intended to represent only the selected embodiments of the present application, and is not intended to limit the scope of protection claimed in the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0056] The present invention provides a method for preparing a TNT / TCPP material for treating printing and dyeing wastewater, comprising the following steps:
[0057] Step S1: Mix NaOH solution with P-25 type TiO 2 The powders are mixed, stirred evenly, and then hydrothermally treated to obtain a first reaction product.
[0058] Step S2, transferring the first reaction product into deionized water, stirring and dispersing it uniformly, and then centrifuging it to remove the supernatant. The precipitate is repeatedly washed with water and centrifuged until the pH value of the washing liquid reaches 7.0.
[0059] Step S3, adding the first reaction product whose washing liquid is neutral after water washing into a dilute hydrochloric acid solution for pickling, and after the pickling is completed, washing again with deionized water until the pH value is 7.0.
[0060] Step S4: drying the first reaction product after washing again, and grinding it thoroughly after drying to obtain TiO 2 Nanotube powder sample.
[0061] Step S5: TiO 2 The nanotube powder sample was placed in anhydrous ethanol and ultrasonicated to make the TiO 2 The nanotube powder samples were uniformly dispersed in anhydrous ethanol.
[0062] Step S6: uniformly disperse the TiO 2 The mixed solution of the nanotube powder sample is added to a uniformly dispersed TCPP ethanol solution, stirred under heating conditions until the ethanol is completely evaporated, and then dried to obtain the TNT / TCPP material.
[0063] Optionally, in step S1, the concentration of the NaOH solution is 10 mol / L.
[0064] Mix NaOH solution with P-25 TiO 2 The specific powder mixing is as follows: 0.8 g of P-25 type TiO 2 The powder was mixed with 50.0 ml of 10 mol / L NaOH solution.
[0065] The temperature of the hydrothermal treatment was 150° C. and the time was 48 hours.
[0066] Optionally, in step S3, the concentration of the dilute hydrochloric acid solution is 0.1 mol / L, and the volume of the added dilute hydrochloric acid is 200 ml.
[0067] Optionally, in step S4, the drying is performed in an oven at a constant temperature of 70°C.
[0068] Optionally, in step S5, TiO 2 The nanotube powder sample was placed in anhydrous ethanol and ultrasonically treated as follows:
[0069] Take 300 mg of TiO 2 The nanotube powder sample was placed in 40 mL of anhydrous ethanol and sonicated for 30 minutes using ultrasound.
[0070] Optionally, in step S6, TCPP and TiO 2 The mass ratio of the nanotube powder sample is 0.1%-1%.
[0071] The stirring was performed at 80°C using a magnetic stirrer.
[0072] The drying treatment was specifically performed by heating in an oven at 80° C. for 10 hours.
[0073] Optionally, in step S1, NaOH solution is mixed with P-25 type TiO 2 The powders are mixed, stirred evenly and then subjected to hydrothermal treatment to obtain a first reaction product, comprising the following steps:
[0074] Step 1.1: Weigh 20.0 g of NaOH using an electronic balance, then dissolve it in 50.0 ml of deionized water to prepare a NaOH solution with a concentration of 10 mol / L under magnetic stirring.
[0075] Step 1.2: Weigh 0.8 g of P-25 TiO 2 The powder was mixed with 50.0 ml of NaOH solution in a Teflon-lined reactor and stirred magnetically for 30 min.
[0076] Step 1.3, remove the magnetic stirrer, seal the reactor, and place the polytetrafluoroethylene liner of the reactor into a stainless steel high-pressure reactor, tighten the lid, place the stainless steel high-pressure reactor in an oven, and perform hydrothermal treatment at 150° C. for 48 hours to obtain a first reaction product.
[0077] Optionally, in step S2, the first reaction product is transferred to deionized water, stirred and dispersed evenly, and then centrifuged to remove the supernatant, and the precipitate is repeatedly washed with water and centrifuged until the pH value of the washing liquid reaches 7.0. Specifically, the stainless steel high-pressure reactor is naturally cooled to room temperature, the first reaction product is taken out and transferred to deionized water, stirred and dispersed evenly to obtain a suspension, the suspension is transferred to a centrifuge tube, 80.0 ml of the suspension is added to each tube, the centrifuge tube is placed in a centrifuge for centrifugal separation, the supernatant is removed, and this process is repeated until the pH value of the washing liquid reaches 7.0.
[0078] Example 1
[0079] This embodiment provides a method for preparing TNT / TCPP materials for treating printing and dyeing wastewater, including two steps of preparing TNT (titanate nanotubes) and preparing TNT / TCPP materials:
[0080] 1.1 Preparation of TNT (titanate nanotubes)
[0081] To prepare TiO 2 Nanotubes, firstly, 20.0 g of NaOH was weighed using an accurate electronic balance, then dissolved in 50.0 ml of deionized water, and a NaOH solution with a concentration of 10 mol / L was prepared under magnetic stirring. Next, 0.8 g of P-25 TiO 2 The powder was mixed with 50.0 ml of the above NaOH solution in a Teflon-lined reactor, and the mixture was magnetically stirred for 30 minutes to ensure thorough mixing. The magnetic stirrer was removed, the reactor was sealed, and the Teflon-lined reactor containing the reaction mixture was placed in a stainless steel autoclave and the lid was tightened. Subsequently, the stainless steel autoclave was placed in an oven and hydrothermally treated at 150°C for 48 hours.
[0082] After the reaction is completed, the stainless steel autoclave is allowed to cool naturally to room temperature. The reaction product is taken out and purified by a water washing procedure. The specific operation is: the material in the polytetrafluoroethylene liner is transferred to deionized water, stirred and dispersed evenly, and then transferred to a centrifuge tube, and 80.0 ml of suspension is added to each tube. The centrifuge tube is placed in a centrifuge for centrifugal separation, the supernatant is removed, and this process is repeated until the pH value of the washing liquid reaches 7.0, indicating that all alkaline impurities have been removed.
[0083] After that, the sample obtained from the last centrifugation was added to 200.0 ml of 0.1 mol / L dilute HCl solution and acid-washed for 3 hours under magnetic stirring to remove possible impurities remaining on the surface. After the acid wash, it was washed again with deionized water to a pH of 7.0 to ensure the neutrality of the sample.
[0084] Finally, the washed samples were dried in an oven at 70 °C to remove all moisture. After drying, the samples were taken out and ground thoroughly to obtain TiO 2 Nanotube powder sample.
[0085] 1.2 TNT / TCPP material preparation
[0086] First, ultrasonic technology was used to disperse the ethanol solution containing different masses of TCPP to achieve complete dispersion of TCPP. The degree of dispersion can be visually determined by light illumination for about 30 minutes. Subsequently, 300 mg of TNT was placed in 40 mL of anhydrous ethanol and ultrasonicated for 30 minutes to achieve uniform dispersion of TNT in the solution.
[0087] Next, the uniformly dispersed TCPP ethanol solution was transferred to the ethanol solution in which TNT was dispersed, and the mixture was stirred at 80°C using a magnetic stirrer until the ethanol was completely evaporated. Finally, the obtained powder was placed in an oven and heated at 80°C for 10 hours to dry it, thereby obtaining a TNT / TCPP material.
[0088] In this embodiment, the above steps can be used to prepare TNT / TCPP materials with different ratios as shown in Table 1.
[0089]
[0090] Example 2 Results Analysis
[0091] In this example, TNT / TCPP materials with different ratios prepared in Example 1 are analyzed.
[0092] 2.1 Scanning electron microscopy analysis (SEM)
[0093] Figure 1 This is the SEM image of the TNT material. It can be found that the TNT material presents a tubular structure, which is consistent with the morphological characteristics of titanate nanotubes. In addition, there are cavities on the surface of the TNT material, which is conducive to the retention of active substances and the redox reaction on the surface of the TNT, which has certain photocatalytic properties.
[0094] Figure 2 This is the SEM image of 1.0% TNT / TCPP material. Compared with the SEM of TNT material, 1.0% TNT / TCPP material still maintains a tubular structure, but there are more gaps between its tubes, which is conducive to electron retention and slows down the speed of electron-hole recombination. Then it is also conducive to the redox reaction of strong oxidizing groups on the surface of the material, improving its photocatalytic performance.
[0095] 2.2 Transmission electron microscopy analysis (TEM)
[0096] Figure 3 This is a TEM image of TNT material. The tubular structure of TNT material can be clearly seen in the image. The outer wall of TNT material is black, and the center is hollow and transparent, which is consistent with the hollow tubular structure of TNT material. Figure 4 After processing the figure a, we get Figure 4 For the stripes in Figure b, we measured the interplanar spacing to be approximately 0.19575nm by taking measurements of the stripes, which is consistent with the interplanar spacing of titanate nanotubes, proving once again that the material is TNT.
[0097] Figure 5 This is the TEM image of the 1.0% TNT / TCPP material. It can be clearly seen in the image that the 1.0% TNT / TCPP material still maintains the tubular structure of the TNT material, and the 1.0% TNT / TCPP material also presents a hollow tubular structure. However, it can be clearly seen that a layer of black TCPP material is attached to the nano-tubular structure of TNT. Figure 6 After processing the figure a, we get Figure 6 The stripes in Figure b were measured to have a crystal plane spacing of approximately 0.3615 nm by taking the amount of the stripes. The results show that the crystal plane spacing of the 1.0% TNT / TCPP material has increased after composite compared to the TNT material.
[0098] 2.3 X-ray diffraction analysis (XRD)
[0099] The curve shows anatase TiO at 2θ = 48.44° 2 The characteristic peaks correspond to the crystal plane indices (101) and (004). Figure 7 The peaks at 2θ=24.32°, 28.36° and 48.36° are characteristic peaks of sodium titanate. This indicates that the Na+ involved in the synthesis reaction plays a role in stabilizing the structure of the nanotubes. P-25 has a characteristic diffraction peak of anatase phase at 2θ=48.44°, and a diffraction peak of rutile type at 2θ=56°. The composite material has a diffraction peak at 2θ=48.44°, indicating that anatase TiO exists in the synthesized TNT / TCPP material. 2 .TiO 2 The photocatalyst made of TCPP loaded on the surface did not change the anatase crystal form, so the photocatalyst TiO 2 It is still in the anatase crystal form, which is more conducive to photocatalysis.
[0100] 2.4 Infrared spectroscopy analysis
[0101] Depend on Figure 8Curve analysis shows that the spectra of titanate nanotubes and their various composite materials in infrared absorption are similar. They are at 3406.6cm -1 The stretching vibration absorption peak of hydroxyl group appears, which is due to the nano-TiO 2 The presence of surface hydroxyl groups. -1 The characteristic absorption peaks of Ti-O-Ti bond appear on the left and right. -1 The left and right are nano-TiO 2 And the characteristic absorption peak of the Ti-O bond of the composite material. When TNT is compounded with different contents of TCPP, the corresponding absorption peaks of different chemical bonds will increase. Among them, the absorption peaks of each bond corresponding to 0.5% TNT / TCPP material are the highest. In photocatalytic applications, high infrared transmittance is usually more conducive to photocatalysis. Because high infrared transmittance means that more infrared light can penetrate the material, which can improve the efficiency of illumination and increase the rate of photocatalytic reaction. High infrared transmittance can also reduce the absorption and reflection of light by the material, thereby improving the utilization efficiency of photocatalytic materials. Therefore, compared with TNT, TNT / TCPP material has been optimized in terms of infrared penetration and has positive benefits.
[0102] exist Fig. 9 In the spectrum of 1715cm -1 and 1290cm -1 It is the stretching vibration of the carboxyl group on the porphyrin ring. 802cm -1 The band at 1562cm is the carboxyl group in the para position of the benzene ring. -1 and 1619cm -1 The absorption bands come from the phenyl groups in the porphyrin ligands, indicating that the porphyrin molecule contains p-carboxyphenyl groups. -1 -1539cm -1 In-plane bending vibration of the CH bond on the benzene ring. 1425cm -1 -1428cm -1 is the in-plane bending vibration of the NH bond.
[0103] 3.5XPS spectrum analysis
[0104] from Fig.10 As can be seen in Figure a, the C peak can usually be decomposed into different chemical bonds, including CC bond, CH bond, CN bond, etc. From the spectrum, it can be seen that the peak values of the C element of TNT and 1.0% TNT / TCPP materials are the same, among which 284.8eV corresponds to the CC bond peak, 286.4eV corresponds to the CN bond peak, and 288.88eV corresponds to the CH bond peak.
[0105] from Fig.10As can be seen in Figure b, the XPS spectrum of the O1s peak of TNT. After curve fitting, the main peak at 530.0eV and the shoulder peak at 532.0eV are obvious, which is mainly attributed to the lattice oxygen (Ti 4+ -O) and surface adsorbed OH (Ti-OH). Due to the increase in the amount of chemically adsorbed water on the TNT surface, the contribution percentage of the Ti-OH component to the total peak after the reaction increased significantly. No new peaks appeared in the figure, indicating that TNT and TCPP did not form new O chemical bonds with each other.
[0106] from Fig.10 As can be seen in Figure c, for the XPS spectrum of Ti 2p, the peaks at 458.78eV and 464.48eV represent Ti 2p 3 / 2 and Ti 2p 1 / 2 From the interval scanning results of titanium element, we can see that there are two peaks at 458.68eV and 464.38eV, which correspond to Ti 2p 3 / 2 and Ti2p 1 / 2 It can be seen that after doping with new materials, no new peaks appear in the XPS spectrum of Ti2p, indicating that TNT and TCPP do not form new Ti bonds. There are no peaks belonging to Ti-C bonds in the figure, indicating that there are no doped carbon atoms in the sample. In addition, there is no peak around 457eV, indicating that there is no Ti in the sample. 3+ Ions exist.
[0107] from Fig.10 As can be seen in Figure d, the main peak at 400.2eV: This peak is usually associated with pyrrole nitrogen. Pyrrole nitrogen is a type of nitrogen atom present in the porphyrin ring. This is consistent with the structure of TCPP, because TCPP is a porphyrin derivative that contains pyrrole nitrogen. The secondary peak at 401.66eV: This peak is usually associated with protonated nitrogen or protonated porphyrin nitrogen. This may be because some nitrogen atoms in TCPP are bound to protons (H+), resulting in an increase in binding energy. The small peak at 408.64eV: This peak is relatively high and may be related to oxidized nitrogen. This peak is generally rare, but it may be due to partial oxidation of the sample during processing or measurement.
[0108] The peak at 400.2eV corresponds to the pyrrolic nitrogen (NC) in the TCPP molecule, which is the main structural feature of TCPP. The peak at 401.66eV corresponds to the protonated pyrrolic nitrogen (N-H+), indicating that some nitrogen atoms in TCPP may be combined with protons to form a protonated form. The peak at 408.64eV may correspond to oxidized nitrogen (NO), indicating that a small amount of oxidized nitrogen compounds may exist in the sample.
[0109] 3.6 Analysis of light response capability
[0110] Since titanium dioxide has unique characteristics in ultraviolet absorption, we tested the ultraviolet absorption rate of P-25, TNT (titanate nanotubes), TCPP (tetrakis (4-carboxyphenyl) porphine) and different ratios of TNT / TCPP materials in different wavelength ranges. Fig.11 It can be seen that the measured materials have a high absorption rate in the wavelength range of 200-300nm, but when it reaches about 300nm, the absorption rate will decrease with the increase of wavelength. P-25, TNT and sodium titanate will continue to decrease with the increase of wavelength, and finally approach zero absorption value. However, although TCPP and TNT / TCPP materials will decrease at 300nm, they will rebound at about 400nm, and have a good absorption effect on ultraviolet rays in the wavelength range of 400-700nm. Through the analysis of the ultraviolet absorption spectrum, it is found that the TNT / TCPP material prepared by the present invention is better than the previous TNT and TiO 2 The material has better UV-visible light absorption performance and has a good absorption rate in most bands.
[0111] By analyzing and calculating the UV-visible absorption spectrum, the UV-visible diffuse reflection is processed using the tangent method, and the data is processed by finding whether the material is a direct gap or an indirect gap. The data is processed using the calculation method in the table below.
[0112] Calculation method
[0113]
[0114] After processing, the data was imported into the origin software for drawing. Fig.12 and Fig.13 It can be found that the TNT / TCPP material prepared by the present invention is better than the traditional TiO 2 The bandgap becomes narrower, which is beneficial to improving the efficiency of photocatalytic reaction.
[0115] 3.7 Fluorescence spectroscopy analysis
[0116] Fig.14 The figure below is a schematic diagram of the fluorescence intensity of TNT and 1.0% TNT / TCPP materials when photogenerated electrons and holes recombine in different bands. It is easy to see from the figure that when the photogenerated electrons and holes recombine, the fluorescence intensity at the peak of the material TNT reaches 1011.6, indicating that the recombination rate of photogenerated electrons and holes at this time is very high. However, the fluorescence intensity at the peak of the material 1.0% TNT / TCPP material is only 393.8, indicating that the 1.0% TNT / TCPP material studied in the present invention will reduce the recombination rate of photogenerated electrons and holes and improve the photocatalytic performance of the material. Fig.14It can be seen that when the material 1.0% TNT / TCPP is in the 400-630nm band, the fluorescence intensity of the photogenerated electrons and holes is almost zero, and it has high photocatalytic performance. When the wavelength exceeds 650nm, the composite material becomes high in recombination rate. The visible light range is 380-750nm, so the newly prepared composite material can show good photocatalytic performance in most bands of visible light, and the recombination rate of photogenerated electrons and holes is very low.
[0117] 3.8 Photocurrent results analysis
[0118] The electrochemical performance of TNT / TCPP materials with different TCPP contents and pure TNT were tested under the same conditions. The results are as follows: Fig.15 It can be seen that the composite material is better than pure TiO 2 It has better separation efficiency, and with the gradual increase of TCPP content, the capacity at different current densities shows an increasing trend. The reason why the composite material shows excellent separation efficiency is not simply a mixture of the two, but because TCPP and TiO 2 The contact forms a heterojunction. Through the effect of the heterojunction interface, it is more compact than direct mixing. TCPP acts as a channel for electron and ion transmission during carrier migration, which increases the conductivity and ion diffusion coefficient of the material, which is beneficial to improving the electrochemical performance of TNT / TCPP materials. The composite material with the best performance we measured is 1.5% TNT / TCPP.
[0119] 3.9 Photocatalytic performance analysis
[0120] The photocatalytic performance of the material was determined by the degradation degree of the rose bengal solution. Because the photocatalytic reaction was preceded by an adsorption process, a dark reaction stage was added to the experiment to compare the difference between the dark reaction and light conditions in order to achieve adsorption equilibrium before the light reaction. The experimental results show that the traditional TNT material is far inferior to the newly prepared TNT / TCPP material in terms of the degradation of rose bengal. Fig.16 It can be seen that in the dark reaction stage, both TNT and TNT / TCPP materials have a certain adsorption effect on the experimental materials.
[0121] In the light reaction stage, Fig.17 and Fig.18It can be seen that the degradation effect of TNT material on rose red solution is poor. Compared with TNT material, TNT / TCPP material has very good degradation effect. However, for TNT / TCPP materials with different ratios, they have different differences in catalytic degradation. Among them, 1.0% TNT / TCPP material has the best degradation effect relatively speaking, and its catalytic efficiency is 35 times that of pure TNT material. Fig.19 It can be clearly seen in the degradation rate bar graph that the 1.0% TNT / TCPP material has the best degradation effect. Therefore, the 1.0% TNT / TCPP material prepared by the present invention has the degradation effect of high-efficiency rose bengal solution and can be applied to the treatment of printing and dyeing wastewater.
[0122] 3.10 Analysis of Electron Paramagnetic Resonance (EPR) Results
[0123] Superoxide radical is abbreviated as O 2 - There are 6 peaks, from left to right, 4 large and 2 small (the peak intensities at positions 1, 2, 4, and 6 are almost the same, and the peak intensities at positions 3 and 5 are lower). Fig. 20 The superoxide spectrum of 1.0% TNT / TCPP material is shown in Figure 2. It can be seen that with the increase of illumination time, the content of superoxide radicals has increased significantly. The increase of superoxide radicals is beneficial to the redox degradation of pollutants in the photocatalytic reaction, and the photocatalytic reaction performance has been significantly improved.
[0124] The hydroxyl free radical is abbreviated as OH. It has 4 peaks. From left to right, the ratio of the peaks is 1:2:2:1. Fig.21 The EPR hydroxyl spectrum of 1.0% TNT / TCPP material is shown in the figure. It can be clearly seen that with the increase of illumination time, the hydroxyl radicals gradually increase. The hydroxyl radicals increase significantly. As a strong oxidizing group in the redox reaction, it is beneficial to the degradation of pollutants in the photocatalytic reaction process and improves the photocatalytic performance.
[0125] Hole (h + ) has three peaks, from left to right, with three equal heights, 1:1:1. Fig. 22 The figure in the middle is the spectrum of holes in 1.0% TNT / TCPP material. It can be clearly seen that with the increase of illumination time, the content of holes is gradually decreasing, which reduces the recombination of electrons and holes and improves the photocatalytic performance.
[0126] The above is only the best specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions within the technical scope disclosed in the present application shall be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing TNT / TCPP material for treating printing and dyeing wastewater, characterized in that: The following steps are involved: Step S1, mixing NaOH solution with P-25 type TiO2 powder, stirring evenly and then performing hydrothermal treatment to obtain a first reaction product; Step S2, transferring the first reaction product into deionized water, stirring and dispersing it uniformly, and then centrifuging it to remove the supernatant, and repeatedly washing and centrifuging the precipitate until the pH value of the washing liquid reaches 7.0; Step S3, adding the first reaction product whose washing liquid is neutral after water washing into a dilute hydrochloric acid solution for pickling, and after the pickling is completed, washing again with deionized water until the pH value is 7.0; Step S4, drying the first reaction product after washing again, and fully grinding it after drying to obtain a TiO2 nanotube powder sample; Step S5, placing the TiO2 nanotube powder sample in anhydrous ethanol and performing ultrasonic treatment so that the TiO2 nanotube powder sample is uniformly dispersed in the anhydrous ethanol; Step S6: adding the uniformly dispersed TiO2 nanotube powder sample mixed solution to the uniformly dispersed TCPP ethanol solution, stirring under heating conditions until the ethanol is completely evaporated, and then drying to obtain the TNT / TCPP material.
2. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 1, characterized in that: In step S1, the concentration of the NaOH solution is 10 mol / L; The mixing of the NaOH solution and the P-25 type TiO2 powder is specifically as follows: 0.8 g of the P-25 type TiO2 powder is mixed with 50.0 ml of the NaOH solution having a concentration of 10 mol / L; The temperature of the hydrothermal treatment is 150° C. and the time is 48 hours.
3. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 2, characterized in that: In step S3, the concentration of the dilute hydrochloric acid solution is 0.1 mol / L, and the volume of the added dilute hydrochloric acid is 200 ml.
4. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 3, characterized in that: In step S4, the drying is performed in an oven at a constant temperature of 70°C.
5. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to any one of claims 1 to 4, characterized in that: In step S5, the TiO2 nanotube powder sample is placed in anhydrous ethanol and subjected to ultrasonic treatment as follows: 300 mg of the TiO2 nanotube powder sample was placed in 40 mL of anhydrous ethanol and subjected to ultrasonic treatment for 30 minutes.
6. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 5, characterized in that: In step S6, the mass ratio of the TCPP to the TiO2 nanotube powder sample is 0.1%-1%; The stirring is carried out by using a magnetic stirrer at a temperature of 80°C; The drying treatment is specifically performed by heating in an oven at 80° C. for 10 hours.
7. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 5, characterized in that: In step S1, the NaOH solution is mixed with the P-25 type TiO2 powder, stirred evenly and then subjected to hydrothermal treatment to obtain a first reaction product, comprising the following steps: 20.0 g of NaOH was weighed using an electronic balance, and then dissolved in 50.0 ml of deionized water to prepare a NaOH solution with a concentration of 10 mol / L under magnetic stirring; Weigh 0.8 g of P-25 TiO2 powder and mix it with 50.0 ml of NaOH solution in a Teflon-lined reactor and stir magnetically for 30 minutes; The magnetic stirrer was removed, the reactor was sealed, and the polytetrafluoroethylene liner of the reactor was placed in a stainless steel autoclave. The lid was tightened, and the stainless steel autoclave was placed in an oven for hydrothermal treatment at 150° C. for 48 hours to obtain the first reaction product.
8. The method for preparing TNT / TCPP material for treating printing and dyeing wastewater according to claim 7, characterized in that: In step S2, the first reaction product is transferred to deionized water, stirred and dispersed uniformly, and then centrifuged to remove the supernatant, and the precipitate is repeatedly washed with water and centrifuged until the pH value of the washing liquid reaches 7.0, specifically: After the stainless steel high-pressure reactor is naturally cooled to room temperature, the first reaction product is taken out and transferred to deionized water, and a suspension is obtained after being stirred and dispersed evenly. The suspension is transferred to a centrifuge tube, 80.0 ml of the suspension is added to each tube, and the centrifuge tube is placed in a centrifuge for centrifugal separation, the supernatant is removed, and this process is repeated until the pH value of the washing liquid reaches 7.
0.
9. A TNT / TCPP material, characterized in that: The TNT / TCPP material is prepared by the method for preparing the TNT / TCPP material for treating printing and dyeing wastewater as described in any one of claims 1 to 8.
10. Use of the TNT / TCPP material according to claim 9 in environmental pollution treatment.