Photocatalytic composite material based on waste building bricks as well as preparation method and application of photocatalytic composite material
By combining construction waste bricks with BiVO4, low-cost and high-efficiency photocatalytic composite materials are prepared, the problems of high cost of traditional photocatalysts and improper treatment of construction waste bricks are solved, and the dual goals of resource utilization and environmental governance are achieved, which has significantly improved the Photocatalytic properties.
Patent Information
- Application Number
- CN202410940388.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
Traditional photocatalysts are expensive to prepare, which limits their large-scale application. Improper treatment of waste bricks on construction has an impact on the environment, and there is a lack of effective utilization solutions.
Combining waste bricks with BiVO4, low-cost photocatalytic composite materials are prepared through ball milling and hydrothermal reaction, improving their photocatalytic performance and stability, and are suitable for pollutant degradation.
It has realized the resource utilization of waste bricks in construction, reduced production costs, significantly improved the photocatalytic reaction performance, is suitable for large-scale production, and plays an important role in environmental governance.
Smart Images

Figure CN118892822A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmentally friendly materials, and specifically relates to a photocatalytic composite material based on building waste bricks, and a preparation method and application thereof. Background Art
[0002] With the acceleration of urbanization, the output of construction waste bricks has increased year by year. How to effectively treat and utilize these construction waste bricks has become an important research topic. Traditional construction waste bricks are mainly made of fired clay and have high strength and stability. However, these waste bricks are usually regarded as construction waste after the building is demolished. Improper treatment will have a serious impact on the environment.
[0003] In recent years, photocatalytic technology has attracted widespread attention due to its high efficiency and stability in environmental governance. Photocatalytic technology can effectively degrade organic pollutants and decompose toxic and hazardous substances under light conditions, and is widely used in water treatment and air purification. Among them, bismuth vanadate (BiVO4), as a highly efficient photocatalyst, has been widely used in the field of photocatalysis due to its narrow band gap and good chemical stability. However, the high preparation cost of traditional photocatalysts limits their large-scale application. Summary of the invention
[0004] In order to achieve efficient resource utilization and environmental protection, combining construction waste bricks with photocatalysts to prepare composite materials with excellent photocatalytic properties has become an innovative solution. This composite material can not only reduce the impact of construction waste bricks on the environment, but also play an important role in environmental governance through its photocatalytic properties. Especially in the degradation of organic pollutants, the photocatalytic activity of these composite materials is significantly better than that of single BiVO4 or construction waste brick materials.
[0005] The present invention aims to provide a photocatalytic composite material based on construction waste bricks and a preparation method thereof. The prepared composite material has low cost, excellent photocatalytic performance and good stability, and is particularly suitable for the field of pollutant degradation. By optimizing the preparation process and material ratio, the present invention further improves the photocatalytic efficiency of the composite material, achieving the dual goals of resource utilization of construction waste bricks and efficient environmental governance.
[0006] The invention provides a photocatalytic composite material based on building waste bricks, which has the advantages of low cost, high photocatalytic performance, good stability and the like as a photocatalytic degradation agent.
[0007] A photocatalytic composite material based on building waste bricks, the preparation method of which comprises the following steps:
[0008] (1) The crushed waste bricks are transferred into a ball mill for ball milling to obtain waste brick powder;
[0009] (2) Bi(NO3)3·5H2O and NH4VO3 are dispersed in nitric acid and deionized water respectively, and stirred evenly. Then, construction waste brick powder is added to the Bi(NO3)3·5H2O solution under stirring. After the solution is continuously stirred, the evenly stirred NH4VO3 solution is added, and then the NH3·H2O solution is added to undergo a hydrothermal reaction. The obtained product is centrifuged and dried to obtain a BiVO4 / construction waste brick composite photocatalytic material.
[0010] Preferably, the above-mentioned photocatalytic composite material based on construction waste bricks is characterized in that, in step (1), the rotation speed of the ball mill is 200 to 400 rpm, and the ball milling time is 10 to 30 min.
[0011] Preferably, the above-mentioned photocatalytic composite material based on construction waste bricks is characterized in that, in step (2), the hydrothermal reaction temperature is 160-200° C., and the hydrothermal time is 8-16 hours.
[0012] Preferably, the above-mentioned photocatalytic composite material based on construction waste bricks is characterized in that, in step (2), the drying is carried out at a temperature of 60 to 100° C. and the drying time is 8 to 12 hours.
[0013] Preferably, the above-mentioned photocatalytic composite material based on construction waste bricks, preparation method and application thereof are characterized in that the photocatalytic composite material based on construction waste bricks is applied in the field of photocatalytic degradation of pollution.
[0014] Preferably, in the above application, methylene blue (MB) is used as the target pollutant to evaluate the photocatalytic performance of the catalyst, and a 300W xenon lamp and a 400nm cut-off filter are used as the visible light source.
[0015] The application method is as follows: 50 mg of the catalyst is added to 50 mL of a 20 mg / L MB solution. The mixture is sonicated for 30 min without light to achieve adsorption / desorption equilibrium of MB on the catalyst. Subsequently, 4 mL of the solution sample is taken every 15 min for 120 min under xenon lamp irradiation. After each sampling, the sample is centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB is measured using a UV-visible spectrophotometer at an absorption wavelength of 660 nm.
[0016] Beneficial effects:
[0017] The present invention provides a photocatalytic composite material based on construction waste bricks and a preparation method thereof, wherein the construction waste bricks are combined with BiVO4 to form a composite photocatalytic material with excellent performance. The addition of construction waste bricks significantly increases the specific surface area of the composite material, provides more active sites, and thus improves the photocatalytic reaction performance. This structure enhances the adsorption capacity and light absorption capacity of the composite material, and improves the photocatalytic activity. At the same time, the use of construction waste bricks as a carrier greatly reduces the production cost, realizes the resource utilization of waste, and reduces the negative impact on the environment. In addition, the preparation process of the composite material is simple, and can be achieved through conventional steps such as ball milling, mixing and hydrothermal reaction, and is suitable for large-scale production. In summary, the photocatalytic composite material based on construction waste bricks of the present invention has significant advantages in performance and cost, shows a wide range of application prospects, and provides a new solution for environmental governance and resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a degradation effect diagram of a photocatalytic composite material based on construction waste bricks prepared in Examples 1 to 5 of the present invention;
[0019] Figure 2 This is a degradation performance diagram of a photocatalytic composite material based on construction waste bricks prepared in Examples 1 to 5 of the present invention;
[0020] Figure 3 This is a degradation rate diagram of a photocatalytic composite material based on construction waste bricks prepared in Examples 1 to 5 of the present invention;
[0021] Figure 4 This is a test chart of the cyclic stability of the composite photocatalytic material prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0022] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0023] Example 1
[0024] A photocatalytic composite material based on construction waste bricks (the mass ratio of BiVO4 to construction waste bricks is 1:4), comprising the following steps:
[0025] Step 1: Transfer the construction waste brick crushed aggregate into a ball mill with a rotation speed of 300 rpm for ball milling for 20 minutes to obtain uniform construction waste brick powder.
[0026] Step 2: Disperse 0.97g Bi(NO3)3·5H2O and 0.234g NH4VO3 into 20mL nitric acid and deionized water respectively, stir evenly, then gradually add 2.592g building waste brick powder into Bi(NO3)3·5H2O solution under stirring and continue stirring. Add the stirred NH4VO3 solution, and finally adjust the pH value of the solution to 7 with NH3·H2O. After stirring evenly, transfer the mixed solution to the lining of a 150mL reactor and place it in an oven at 180°C for 12 hours of hydrothermal reaction. After the reaction is completed, collect the precipitate and wash it repeatedly with ethanol and deionized water, centrifuge the washed product, and dry it at 80°C to obtain the BiVO4 / building waste brick composite photocatalytic material.
[0027] Step 3: To evaluate the photocatalytic performance of the catalyst, 50 mg of the catalyst was added to 50 mL of a 20 mg / L MB solution. The mixture was ultrasonically treated for 30 min without light to achieve the adsorption / desorption equilibrium of MB on the catalyst surface. Subsequently, 4 mL of the solution sample was taken every 15 min for 120 min under irradiation with a 300 W xenon lamp (equipped with a 400 nm cutoff filter). After each sampling, the sample was centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB was determined using a UV-Vis spectrophotometer at an absorption wavelength of 660 nm.
[0028] Example 2
[0029] A photocatalytic composite material based on construction waste bricks (the mass ratio of BiVO4 to construction waste bricks is 1:2), comprising the following steps:
[0030] Step 1: Transfer the construction waste brick crushed aggregate into a ball mill with a rotation speed of 300 rpm for ball milling for 20 minutes to obtain uniform construction waste brick powder.
[0031] Step 2: Disperse 1.94g Bi(NO3)3·5H2O and 0.468g NH4VO3 into 20mL nitric acid and deionized water respectively, stir evenly, then gradually add 2.592g building waste brick powder into Bi(NO3)3·5H2O solution under stirring and continue stirring. Add the stirred NH4VO3 solution, and finally adjust the pH value of the solution to 7 with NH3·H2O. After stirring evenly, transfer the mixed solution to the lining of a 150mL reactor and place it in an oven at 180°C for 12 hours of hydrothermal reaction. After the reaction is completed, collect the precipitate and wash it repeatedly with ethanol and deionized water, centrifuge the washed product, and dry it at 80°C to obtain the BiVO4 / building waste brick composite photocatalytic material.
[0032] Step 3: To evaluate the photocatalytic performance of the catalyst, 50 mg of the catalyst was added to 50 mL of a 20 mg / L MB solution. The mixture was ultrasonically treated for 30 min without light to achieve the adsorption / desorption equilibrium of MB on the catalyst surface. Subsequently, 4 mL of the solution sample was taken every 15 min for 120 min under irradiation with a 300 W xenon lamp (equipped with a 400 nm cutoff filter). After each sampling, the sample was centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB was determined using a UV-Vis spectrophotometer at an absorption wavelength of 660 nm.
[0033] Example 3
[0034] A photocatalytic composite material based on construction waste bricks (the mass ratio of BiVO4 to construction waste bricks is 1:1), comprising the following steps:
[0035] Step 1: Transfer the construction waste brick crushed aggregate into a ball mill with a rotation speed of 300 rpm for ball milling for 20 minutes to obtain uniform construction waste brick powder.
[0036] Step 2: Disperse 1.94g Bi(NO3)3·5H2O and 0.468g NH4VO3 into 20mL nitric acid and deionized water respectively, stir evenly, then gradually add 1.296g building waste brick powder into Bi(NO3)3·5H2O solution under stirring and continue stirring. Add the stirred NH4VO3 solution, and finally adjust the pH value of the solution to 7 with NH3·H2O. After stirring evenly, transfer the mixed solution to the lining of a 150mL reactor and place it in an oven at 180°C for 12 hours of hydrothermal reaction. After the reaction is completed, collect the precipitate and wash it repeatedly with ethanol and deionized water, centrifuge the washed product, and dry it at 80°C to obtain the BiVO4 / building waste brick composite photocatalytic material.
[0037] Step 3: To evaluate the photocatalytic performance of the catalyst, 50 mg of the catalyst was added to 50 mL of a 20 mg / L MB solution. The mixture was ultrasonically treated for 30 min without light to achieve the adsorption / desorption equilibrium of MB on the catalyst surface. Subsequently, 4 mL of the solution sample was taken every 15 min for 120 min under irradiation with a 300 W xenon lamp (equipped with a 400 nm cutoff filter). After each sampling, the sample was centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB was determined using a UV-Vis spectrophotometer at an absorption wavelength of 660 nm.
[0038] Example 4
[0039] A photocatalytic composite material based on construction waste bricks (the mass ratio of BiVO4 to construction waste bricks is 2:1), comprising the following steps:
[0040] Step 1: Transfer the construction waste brick crushed aggregate into a ball mill with a rotation speed of 300 rpm for ball milling for 20 minutes to obtain uniform construction waste brick powder.
[0041] Step 2: Disperse 1.94g Bi(NO3)3·5H2O and 0.468g NH4VO3 into 20mL nitric acid and deionized water respectively, stir evenly, then gradually add 0.648g building waste brick powder into Bi(NO3)3·5H2O solution under stirring and continue stirring. Add the stirred NH4VO3 solution, and finally adjust the pH value of the solution to 7 with NH3·H2O. After stirring evenly, transfer the mixed solution to the lining of a 150mL reactor and place it in an oven at 180°C for 12 hours of hydrothermal reaction. After the reaction is completed, collect the precipitate and wash it repeatedly with ethanol and deionized water, centrifuge the washed product, and dry it at 80°C to obtain the BiVO4 / building waste brick composite photocatalytic material.
[0042] Step 3: To evaluate the photocatalytic performance of the catalyst, 50 mg of the catalyst was added to 50 mL of a 20 mg / L MB solution. The mixture was ultrasonically treated for 30 min without light to achieve the adsorption / desorption equilibrium of MB on the catalyst surface. Subsequently, 4 mL of the solution sample was taken every 15 min for 120 min under irradiation with a 300 W xenon lamp (equipped with a 400 nm cutoff filter). After each sampling, the sample was centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB was determined using a UV-Vis spectrophotometer at an absorption wavelength of 660 nm.
[0043] Example 5
[0044] A photocatalytic composite material based on construction waste bricks (the mass ratio of BiVO4 to construction waste bricks is 1:4), comprising the following steps:
[0045] Step 1: Transfer the construction waste brick crushed aggregate into a ball mill with a rotation speed of 300 rpm for ball milling for 20 minutes to obtain uniform construction waste brick powder.
[0046] Step 2: Disperse 1.94g Bi(NO3)3·5H2O and 0.468g NH4VO3 into 20mL nitric acid and deionized water respectively, stir evenly, then gradually add 0.324g building waste brick powder into Bi(NO3)3·5H2O solution under stirring and continue stirring. Add the stirred NH4VO3 solution, and finally adjust the pH value of the solution to 7 with NH3·H2O. After stirring evenly, transfer the mixed solution to the lining of a 150mL reactor and place it in an oven at 180°C for 12 hours of hydrothermal reaction. After the reaction is completed, collect the precipitate and wash it repeatedly with ethanol and deionized water, centrifuge the washed product, and dry it at 80°C to obtain the BiVO4 / building waste brick composite photocatalytic material.
[0047] Step 3: To evaluate the photocatalytic performance of the catalyst, 50 mg of the catalyst was added to 50 mL of a 20 mg / L MB solution. The mixture was ultrasonically treated for 30 min without light to achieve the adsorption / desorption equilibrium of MB on the catalyst surface. Subsequently, 4 mL of the solution sample was taken every 15 min for 120 min under irradiation with a 300 W xenon lamp (equipped with a 400 nm cutoff filter). After each sampling, the sample was centrifuged in a centrifuge at 6000 rpm for 5 min. The content of MB was determined using a UV-Vis spectrophotometer at an absorption wavelength of 660 nm.
[0048] The present invention will be further described below in conjunction with the accompanying drawings and Examples 1 to 5:
[0049] Figure 1 The results show the effect of the photocatalytic composite material based on construction waste bricks prepared in Examples 1 to 5 of the present invention in the photocatalytic degradation of MB. Under visible light irradiation conditions, the degradation rates of Examples 1 to 5 reached 78.52%, 82.5%, 93.84%, 90.41% and 86.14%, respectively, and it can be seen that Example 3 has the best degradation effect.
[0050] Figure 2 The photocatalytic degradation performance diagram of a photocatalytic composite material based on construction waste bricks prepared in Examples 1 to 5 of the present invention shows the degradation performance of the photocatalytic composite materials prepared in Examples 1 to 5 under light irradiation, and it can be seen that Example 3 has the best degradation performance.
[0051] Figure 3 The photocatalytic degradation rate diagram of a photocatalytic composite material based on building waste bricks prepared in Examples 1 to 5 of the present invention. Under visible light irradiation conditions, the degradation rates of Examples 1 to 5 reached 0.01236 min -1 、0.01265min -1 、0.02124min -1 、0.01811min-1 and 0.01574min -1 Among them, Example 3 has the highest degradation rate, which further verifies that Example 3 has excellent photocatalytic performance.
[0052] Figure 4 This is a cyclic stability test diagram of a photocatalytic composite material based on construction waste bricks prepared in Example 3 of the present invention. The results show that the test sample has very excellent stability. In summary, the photocatalytic composite material based on construction waste bricks prepared in this embodiment has excellent photocatalytic degradation performance of pollutants.
[0053] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a photocatalytic composite material, characterized in that: The following steps are involved: (1) crushing the construction waste and then ball milling it to obtain construction waste powder; (2) A nitric acid dispersion of Bi(NO3)3·5H2O, a deionized water dispersion of NH4VO3, an NH3·H2O solution and the construction waste powder are mixed, subjected to a hydrothermal reaction, centrifuged and dried to obtain the photocatalytic composite material.
2. The preparation method according to claim, characterized in that: During the ball milling in step (1), the rotation speed is 200 to 400 rpm and the ball milling time is 10 to 30 min.
3. The preparation method according to claim 1, characterized in that: In step (2), Bi(NO3)3·5H2O and NH4VO3 are dispersed in nitric acid and deionized water respectively, and stirred evenly. Then, the construction waste powder is added to the Bi(NO3)3·5H2O solution while stirring in a water bath stirring pot. After the solution is continuously stirred, the evenly stirred NH4VO3 solution is added, and then the NH3·H2O solution is added.
4. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the hydrothermal reaction is 160-200° C., and the hydrothermal time is 8-16 hours.
5. The preparation method according to claim 1, characterized in that: The drying temperature in step (2) is 60-100° C. and the drying time is 8-12 hours.
6. A photocatalytic composite material prepared by the preparation method according to any one of claims 1 to 5.
7. The photocatalytic composite material according to claim 6, characterized in that: The construction waste includes construction waste bricks.
8. Use of the photocatalytic composite material according to claim 6 or 7 in photocatalytic degradation of pollution.
9. A method for degrading methylene blue pollution, characterized in that: Under the action of light, the photocatalytic composite material according to claim 6 or 7 is mixed with pollutants to cause a photocatalytic reaction.
Citation Information
Patent Citations
Functional construction waste material and recycling preparation method thereof
CN109158405A
Composite photocatalytic material containing construction waste micro-powder and preparation method of composite photocatalytic material
CN113769724A
Visible light photocatalytic material for degrading formaldehyde and preparation method thereof
CN118268018A
New synthetic method for fine powder of visible light-responsive bismuth vanadate, photocatalyst of fine powder of new visible light-responsive bismuth vanadate and cleaning method using the same
JP2004024936A
Cited By
Photocatalytic composite material based on fly ash as well as preparation method and application of photocatalytic composite material
CN119633801A
Construction waste-based adsorption and passivation bifunctional water treatment agent and preparation method thereof
CN121085360A