Catalytic oxidation ceramsite as well as preparation method and application thereof

Through the granulation of dry sludge powder and the transition metal salt modification and calcining process, efficient catalytic oxidized ceratops are prepared, which solves the problems of sludge resource utilization and high cost of ceratops, and realizes high value-added utilization and environmentally friendly ceratops production .

CN118892835AInactive Publication Date: 2024-11-05ZHONGKE (YIXING) NEW MATERIAL RES CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410941049.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, sludge has not been fully resourced and the high cost of ceram production, especially the high cost of catalytic oxidants and environmental pollution in sewage treatment.

Method used

Using dry sludge powder as raw material, catalytic oxidized ceramates with high porosity, hardness and compressive resistance are prepared through granulation, transition metal salt solution modification and calcining process under the protection of inert gas, avoiding the addition of additional ore powder and powder. Materials such as coal ash reduce production costs.

Benefits of technology

The high added value utilization of sludge is achieved, and the production cost of ceratops is reduced. The catalytic oxidized ceratops have the performance of rapidly degrading organic pollutants under ozone aeration conditions, which is environmentally friendly and simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892835A_ABST
    Figure CN118892835A_ABST
Patent Text Reader

Abstract

The invention discloses catalytic oxidation ceramsite as well as a preparation method and application thereof. The preparation method of the ceramsite comprises the following steps: granulating a mixture containing dry sludge powder, a binder and a solvent to obtain pellets; soaking the spherical particles in a transition metal salt solution or spraying the transition metal salt solution on the surfaces of the spherical particles, and drying to obtain modified spherical particles; under the protection of inert gas, the modified spherical particles are calcined for 0.5-6 h at the temperature of 900-1200 DEG C, and catalytic oxidation ceramsite is obtained; or, granulating the mixture of the dry sludge powder and the solvent to obtain pellets; spraying a transition metal salt solution on the surfaces of the pellets, and drying to obtain modified pellets; and under the protection of inert gas, calcining the modified spherical particles at 900-1200 DEG C for 0.5-6 hours to obtain the catalytic oxidation ceramsite. The prepared catalytic oxidation ceramsite has good activity and stability, and can quickly degrade organic pollutants under the condition of ozone aeration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention specifically relates to catalytic oxidation ceramsite and a preparation method and application thereof. Background Art

[0002] The high content of organic matter in lake and river silt has caused the water to remain eutrophic for a long time, leading to the outbreak of blue algae and the destruction of the ecological environment. Taking Taihu Lake as an example, dredging operations began in 2007, and the total amount of dredging in 13 years was 23 million m 3 , dredging cost 200 yuan / m 3 However, compared to 1.915 billion m 3 In terms of the total siltation, it is still the tip of the iceberg. In addition, the current large-scale natural solidification and stacking of sludge takes up a large area, the odor lasts for a long time, and it cannot generate economic value.

[0003] In order to increase the added value of sludge and turn waste into treasure, a series of resource utilization schemes have been developed. According to the different components and properties of sludge, it can be roughly divided into three uses: (1) fertile floating mud can be used as backfill soil for landscaping and vegetable bases (a method for preparing planting soil by solidifying and improving sludge, Chinese patent application CN 116491394A); (2) sludge with higher hardness can be used as abandoned fish pond and mine repair soil (a method and equipment for preparing mine repair materials using river sludge, Chinese patent application CN 113860945A); (3) Slightly harder sludge can be processed into ecological building materials (a method for preparing high-strength thermal insulation bricks using riverbed sludge, Chinese patent application CN 115304351A). Although these three treatment methods provide a way out for the resource utilization of sludge, the added value is still low and it is impossible to truly turn waste into treasure and create value.

[0004] Preparing sludge into ceramsite is an effective way to promote the resource utilization of sludge. Chinese patent document CN113816761A discloses a composite ceramsite, which is obtained by calcining raw materials using biomass and / or natural gas as fuel, and the raw materials include silt, shale and a binder; Chinese patent document CN102515831A discloses a cylindrical attapulgite riverbed silt ceramsite, which uses 1-10% high-viscosity attapulgite clay powder, 5-25% attapulgite clay tailings powder, 5-20% red bentonite powder, 45-65% riverbed sludge, 5-20% fly ash and 1-10% sawdust powder as ingredients; However, these existing preparation methods generally require the additional addition of some mineral powder, fly ash, shale and other substances, which increases the preparation cost of ceramsite.

[0005] Sewage plants widely use advanced oxidation technology to treat organic pollutants in sewage, and the core component is heterogeneous catalyst. The current market price of ceramsite catalyst is 15,000-20,000 yuan / ton, which is relatively expensive. Therefore, from an economic and environmental perspective, it is urgent to develop green preparation technology for the resource utilization of waste pollutants and realize low-cost, green and environmentally friendly ceramsite preparation with high catalytic performance. Summary of the invention

[0006] The technical problem solved by the present invention is to overcome the defects of the prior art that the sludge cannot be fully utilized as a resource and the production cost of ceramsite is high, and to provide a catalytic oxidation ceramsite and a preparation method and application thereof. The preparation method of the present invention is energy-saving and environmentally friendly, and does not generate pollution during the production process. It not only realizes the waste utilization of sludge, but also reduces the production cost of ceramsite; the prepared catalytic oxidation ceramsite has good activity and stability, and can quickly degrade organic pollutants under ozone aeration conditions.

[0007] The present invention uses dry sludge powder as raw material, and does not require the addition of mineral powder, fly ash, shale and other materials. Through granulation, transition metal salt solution modification and calcination, catalytic oxidation ceramsite with high porosity, hardness, compression resistance and excellent degradation performance for organic pollutants can be obtained, which greatly reduces the production cost of ceramsite.

[0008] The present invention solves the above technical problems through the following technical solutions:

[0009] The present invention provides a method for preparing catalytic oxidation ceramsite, which comprises the following steps:

[0010] Method 1:

[0011] Granulating a mixture containing dry sludge powder, a binder and a solvent to obtain pellets, wherein the mass ratio of the dry sludge powder to the binder is 1000:(0.5-40); then soaking the pellets in a transition metal salt solution or spraying the transition metal salt solution on the surface of the pellets, and drying to obtain modified pellets; calcining the modified pellets at 900-1200° C. for 0.5-6 h under the protection of an inert gas to obtain the catalytic oxidation ceramsite;

[0012] Or, method 2:

[0013] The mixture of dry sludge powder and solvent is granulated to obtain pellets; a transition metal salt solution is sprayed on the surface of the pellets, and after drying, modified pellets are obtained; under the protection of inert gas, the modified pellets are calcined in the range of 900-1200° C. for 0.5-6h to obtain the catalytic oxidation ceramsite.

[0014] In the present invention, the moisture content of the dried sludge powder may be 1%-5%, for example 3%. The moisture content is calculated by the formula: mass moisture content (%) = (m2-m1) / m1*100%, m1 is the dry weight of the substance, and m2 is the wet weight of the substance.

[0015] In the present invention, the particle size D50 of the dried sludge powder may be 15-25 μm, for example, 19.9 μm.

[0016] In the present invention, the dried sludge powder can generally be obtained by dehydrating and crushing the raw sludge. The raw sludge can be the sludge at the bottom of Taihu Lake.

[0017] In the present invention, the solvent may be one or more of deionized water, methanol, ethanol and isopropanol, such as deionized water.

[0018] In the present invention, the ratio of the mass of the dry sludge powder to the volume of the solvent is preferably 100 g:(70-80) mL, for example 100 g:75 mL.

[0019] In the present invention, the binder may be one or more of sodium carboxymethyl cellulose, sodium carboxymethyl starch, polyacrylic acid and polyacrylamide. The weight average molecular weight of the polyacrylamide may be 1*10 6 -2*10 7 , for example 2*10 6 -1.4*10 7 The average molecular weight of the polyacrylic acid may be M w =1*10 6 -1*10 7 , for example 4*10 6 When the binder is sodium carboxymethyl cellulose and / or sodium carboxymethyl starch, the mass ratio of the dry sludge powder to the binder may be 100:(0.5-4), preferably 100:(0.5-2), for example 100:1. When the binder is polyacrylic acid and / or polyacrylamide, the mass ratio of the dry sludge powder to the binder may be 1000:(0.5-4), for example 1000:1 or 1000:2.

[0020] In the present invention, the granulation can be carried out on a granulation plate or a roller extrusion granulator. The operation and conditions of the granulation can be conventional in the art, for example, the size of the pellets can be controlled by adjusting the mesh number of the screen on the granulation plate. The mesh number of the screen can be 4-7 meshes.

[0021] In the present invention, the particle size of the spherical particles may be 3-10 mm, preferably 3-5 mm.

[0022] In the present invention, the metal in the transition metal salt solution includes one or more of Fe, Mn and Co. The transition metal salt is preferably one or more of metal citrate, metal acetate, metal acetylacetonate, metal chloride, metal nitrate and metal sulfate. In a specific embodiment, the transition metal salt solution is a ferric citrate solution.

[0023] In the present invention, the concentration of the transition metal salt solution may be 0.1-1M, such as 0.2M or 0.5M.

[0024] In the present invention, the soaking time may be 5-10 seconds, for example 8 seconds. During the soaking, the volume of the transition metal salt solution is generally sufficient to completely cover the pellets.

[0025] In some embodiments, the soaking preferably comprises the following step: soaking the pellets in a 0.2M ferric citrate solution for 5-10 seconds.

[0026] In the present invention, the spraying operation can be conventional in the art, for example, the transition metal salt solution is sprayed on the surface of the pellets using a spray pot or a coating machine. The spray pot can be a conventional spray pot in the art, such as a pumpkin spray pot. During the spraying, the ratio of the mass of the pellets to the volume of the transition metal salt solution is preferably 100 g: (1.5-3) mL, for example 100 g: 2 mL.

[0027] In some embodiments, the spraying comprises the following steps: using a spray pot to spray 0.2M ferric citrate solution on the surface of the pellets, and the ratio of the mass of the pellets to the volume of the ferric citrate solution is preferably 100 g: (1.5-3) mL.

[0028] In the present invention, the drying method can be conventional in the art, such as drying. The drying temperature can be 100-200°C, such as 120°C.

[0029] In the present invention, the inert gas may be conventional in the art, such as nitrogen or argon.

[0030] In the present invention, the calcination temperature is preferably 1000-1100°C, such as 1000°C or 1100°C.

[0031] In the present invention, the calcination time is preferably 1-4 hours, such as 1 hour or 3 hours.

[0032] The invention also provides a catalytic oxidation ceramsite prepared by the above method.

[0033] In the present invention, the catalytic oxidation ceramsite may be in the shape of a regular sphere or an ellipsoid.

[0034] The present invention also provides an application of the catalytic oxidation ceramsite as described above in sewage treatment.

[0035] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0036] The reagents and raw materials used in the present invention are commercially available.

[0037] The positive and progressive effects of the present invention are:

[0038] (1) The ceramsite catalyst prepared by the present invention has high porosity, hardness, and compressive strength, and has excellent performance in degrading organic pollutants;

[0039] (2) The present invention uses lake and river sludge as raw material to prepare oxidized ceramsite catalyst, which effectively consumes sludge solid waste, reduces secondary pollution caused by the accumulation process, and realizes high added value utilization of sludge;

[0040] (3) The present invention uses lake and river sludge as raw materials to prepare advanced oxidation ceramsite catalysts, saving the purchase costs of ceramsite and metal precursors, and effectively reducing production costs;

[0041] (4) The preparation process of the present invention is simple and easy to operate, which is conducive to large-scale production. The production process does not produce toxic and harmful by-products and does not cause environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Part (a) is a photograph of dry sludge powder; Figure 1 Part (b) is the XRD pattern of the dried sludge powder; Figure 1 Part (c) is the EDX spectrum of the dried sludge powder;

[0043] Figure 2 A photograph of the catalytic oxidation ceramsite prepared in Example 1;

[0044] Figure 3 The SEM image of the catalytic oxidation ceramsite prepared in Example 1;

[0045] Figure 4 This is a photo of the ceramsite prepared in Comparative Example 2;

[0046] Figure 5 Part (a) is a graph showing the changes of the pellets obtained by granulation in Example 2 after being immersed in water for 15 minutes; Figure 5 Part (b) is a graph showing the changes of the pellets obtained by granulation in Example 1 after being immersed in water for 15 minutes;

[0047] Figure 6 The pollutant degradation rate and quality change diagram of the catalytic oxidation ceramsite prepared in Example 1 after ten cycles of use;

[0048] Figure 7 Part (a) is a graph showing the degradation rate of simulated pollutants by the catalytic oxidation ceramsite prepared in Example 1 under different pH environments; Figure 7 Part (b) is a graph showing the degradation rate of the catalytic oxidation ceramsite prepared in Example 1 for different simulated pollutants;

[0049] Figure 8 Part (a) is a graph showing the degradation rate and quality change of organic matter after the catalytic oxidation ceramsite prepared in Comparative Example 1 was recycled for ten times; Figure 8 Part (b) is a graph showing the degradation rate and quality change of organic matter after the catalytic oxidation ceramsite prepared in Comparative Example 2 was recycled for ten times; Figure 8 Part (c) is a graph showing the organic matter degradation rate and mass change after the catalytic oxidation ceramsite catalyst prepared in Comparative Example 4 was recycled for ten times;

[0050] Fig. 9 Part (a) is a photo of the ceramsite prepared in Comparative Example 3 after 8 hours of aeration; Fig. 9 Part (b) is a photograph of the expanded clay prepared in Example 1 after 8 hours of aeration. DETAILED DESCRIPTION

[0051] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0052] The raw sludge used in the following embodiments and comparative examples is the Taihu Lake bottom sludge extracted through a closed pipeline by a suction dredger. Before use, the raw sludge is first dehydrated by exposure to the sun at a shore sludge yard, and then the blocky sludge is crushed by a sand and gravel crusher to obtain a dry sludge powder with a water content of 3% and a particle size D50 of 19.9 μm.

[0053] Example 1

[0054] Take 200 grams of dry sludge powder, add 2 grams of sodium carboxymethyl cellulose and 150 milliliters of deionized water, stir evenly, use a granulation plate with a mesh size of 6 to make 3-5 mm pellets; soak the prepared pellets in 200 mL of 0.2 mol / L ferric citrate solution for 8 seconds and then filter them, dry the filtered pellets at 120°C in a blast oven for 12 hours, then transfer the dried pellets to a tubular furnace, calcine at 1000°C for 1 hour in a nitrogen atmosphere, and naturally cool to room temperature to obtain catalytic oxidation ceramsite.

[0055] Example 2

[0056] Take 200 grams of dry sludge powder and 150 milliliters of deionized water, stir evenly, and use a granulation plate to make 3-5 mm pellets; according to the standard of spraying 2 mL of 0.2 mol / L ferric citrate solution per 100 g of pellets, use a spray pot to spray the ferric citrate solution on the surface of the pellets, and dry the sprayed pellets in a blast oven at 120°C for 12 hours. Then transfer the dried pellets to a tubular furnace, calcine at 1000°C for 1 hour under a nitrogen atmosphere and inert gas, and naturally cool to room temperature to obtain catalytic oxidation ceramsite.

[0057] Example 3

[0058] Compared with Example 1, except that 2 grams of sodium carboxymethyl cellulose is replaced by 0.2 grams of polyacrylamide (Aladdin, molecular weight Mw: 2 million-14 million), the other operations and conditions are the same as those in Example 1.

[0059] Example 4

[0060] Compared with Example 1, except that 2 grams of sodium carboxymethyl cellulose was replaced by 0.2 grams of polyacrylic acid (Aladdin, average molecular weight Mv is 4000000), the other operations and conditions were the same as those in Example 1.

[0061] Example 5

[0062] Compared with Example 2, except that the calcination temperature is adjusted to 900°C, the other operations and conditions are the same as those of Example 2.

[0063] Example 6

[0064] Compared with Example 2, except that the calcination temperature is adjusted to 1100° C., the other operations and conditions are the same as those of Example 2.

[0065] Example 7

[0066] Compared with Example 2, except that the calcination time is adjusted to 0.5 h, the other operations and conditions are the same as those in Example 2.

[0067] Example 8

[0068] Compared with Example 2, except that the calcination time is adjusted to 3 hours, the other operations and conditions are the same as those in Example 2.

[0069] Comparative Example 1

[0070] Take 200 grams of dry sludge powder, add 2 grams of sodium carboxymethyl cellulose and 150 milliliters of deionized water, stir evenly, and use a granulation plate to make 3-5 mm pellets; transfer the prepared pellets to a tubular furnace, calcine at 1000°C for 1 hour under a nitrogen atmosphere to obtain catalytic oxidation ceramsite.

[0071] Comparative Example 2

[0072] Compared with Example 1, except that the atmosphere during the calcination process was changed to air, the other operations and conditions were the same as those in Example 1. The prepared ceramsite product was red pellets ( Figure 4 ), this is because during the calcination process, the organic matter comes into contact with oxygen at high temperature and is converted into carbon dioxide, and the iron ions are all converted into iron oxide.

[0073] Comparative Example 3

[0074] Compared with Example 1, except that the calcination temperature during the calcination process is set to 800° C., the other operations and conditions are the same as those of Example 1.

[0075] Comparative Example 4

[0076] Compared with Example 1, except that the 0.2 mol / L ferric citrate solution was replaced by a 0.2 mol / L citric acid solution, the other operations and conditions were the same as those in Example 1.

[0077] Effect Example

[0078] (1) Morphology and element content

[0079] Figure 1 Part (a) is a photograph of dry sludge powder; Figure 1 Part (b) is the XRD pattern of the dried sludge powder; Figure 1 Part (c) is the EDX spectrum of the dry sludge powder. According to the EDX spectrum analysis, calculated by the mass percentage of each element in the dry sludge powder, it can be seen that the dry sludge powder contains 53.83% O, 19.12% Si, 16.58% C, 6.36% Al, 1.87% Fe, 0.73% K, 0.77% Mg, 0.39% Ca and 0.35% Na.

[0080] Figure 2 A photograph of the catalytic oxidation ceramsite prepared in Example 1; Figure 3 This is a SEM image of the catalytic oxidation ceramsite prepared in Example 1. According to the SEM image, a large number of pore structures ( Figure 3 The red circle indicates that the specific surface area and porosity of the ceramsite are increased, which is conducive to exposing more active sites. Figure 4 This is a photo of the ceramsite prepared in Comparative Example 2.

[0081] according to Figure 5 It can be seen that in the preparation process of Example 2, since sodium carboxymethyl cellulose was not added, the granules prepared by granulation were easily soluble in water, and the ferric citrate ( Figure 5a); and the pellets prepared by granulation with the addition of a binder, sodium carboxymethyl cellulose, in Example 1 can remain stable in water and can be modified by immersion or spraying of ferric citrate ( Figure 5 b).

[0082] (2) Density test of catalytic oxidation ceramsite

[0083] Actual density test method: add a certain mass of ceramsite into a measuring cylinder filled with water, read the scale change value, calculate the actual volume of the ceramsite, and then calculate the actual density;

[0084] Method for testing bulk strength: Add a certain mass of expanded clay into a measuring cylinder, read the scale, and calculate the density.

[0085] The actual density of the ceramsite prepared in Example 1 is 2.15*10 3 kg / m3, the bulk density is 0.99*10 3 kg / m3, a single ceramsite can withstand a pressure of more than 200N.

[0086] (3) Wastewater treatment

[0087] A series of identical simulated wastewater A was prepared: 1.5 L of 50 mg / L phenol, and 0.2 mL of 30% (mass fraction) hydrogen peroxide was added;

[0088] match Prepare a series of simulated wastewater B with different pH values: 1.5 L of 50 mg / L phenol, add 0.2 mL of 30% (mass fraction) hydrogen peroxide, and adjust the pH value to 5-9 using 1 M nitric acid solution or 1 M sodium hydroxide solution;

[0089] A series of simulated wastewater C containing different types of organic pollutants were prepared: compared with simulated wastewater A, phenol was replaced by triadimefon, paclobutrazol, diisobutyl phthalate, oxalic acid, bisphenol A, and potassium hydrogen phthalate, respectively, and the initial COD of the simulated wastewater containing each organic pollutant was controlled to be 120 mg / L;

[0090] During the test, 200g of the catalytic oxidation ceramsite prepared in Examples 1-8 and Comparative Examples 1-4 were added to the prepared simulated wastewater A, and simulated wastewater tests were carried out in an aeration tower. Ozone was continuously introduced during the test, with an ozone concentration of 12mg / L, an air flow rate of 0.5L / min, and ventilation for 1.5 hours. The COD of the simulated wastewater before and after the test was tested according to "HJ 828-2017 Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method", and the test results are shown in Tables 2 and Figure 6 , Figure 8According to the experimental results, the ceramsite prepared in the embodiment has a good degradation effect on phenol, and the structure is stable during the aeration process. After 10 cycles, it still has a high degradation rate and less mass loss. In addition, a series of 200g of catalytic oxidation ceramsite prepared in Example 1 were weighed and added to the prepared simulated wastewater B and simulated wastewater C, and tested according to the above method. The test results are shown in Figure 7 According to the test results, the prepared ceramsite has stable catalytic degradation performance at different pH values, and has achieved good degradation effects on different organic pollutants. The average organic matter degradation rate is 73.1% and the mass loss is 0.18 grams.

[0091] Cyclic experiment test process: Test according to the above test process. After each test, filter out the ceramsite, wash and dry it with deionized water, and replace it with simulated wastewater for testing.

[0092] According to the test results, since comparative example 1 is not modified with metal salts and comparative example 2 is calcined in air, the degradation effect of the prepared ceramsite is poor and the quality loss is large during the first cycle.

[0093] After 1.5 hours of ozone aeration, the COD of the ceramsite prepared in Comparative Example 3 decreased by 77%. After 8 hours of long-term aeration, the ceramsite showed obvious dissolution ( Fig. 9 a); as a comparison, the ceramsite product prepared by calcining at 1000°C in Example 1 was aerated for 8 hours and still had good stability ( Fig. 9 b).

[0094] Since comparative example 4 is modified with citric acid without metal ions, the degradation effect of the prepared ceramsite is poor during the first cycle.

[0095] Table 2

[0096]

[0097] Note: COD degradation rate = 1-initial COD / final COD.

[0098] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.

Claims

1. A method for preparing catalytic oxidation ceramsite, characterized in that: It includes the following steps: Method 1: Granulating a mixture containing dry sludge powder, a binder and a solvent to obtain pellets, wherein the mass ratio of the dry sludge powder to the binder is 1000:(0.5-40); then soaking the pellets in a transition metal salt solution or spraying the transition metal salt solution on the surface of the pellets, and drying to obtain modified pellets; calcining the modified pellets at 900-1200° C. for 0.5-6 h under the protection of an inert gas to obtain the catalytic oxidation ceramsite; Or, method 2: The mixture of dry sludge powder and solvent is granulated to obtain pellets; a transition metal salt solution is sprayed on the surface of the pellets, and after drying, modified pellets are obtained; under the protection of inert gas, the modified pellets are calcined in the range of 900-1200° C. for 0.5-6h to obtain the catalytic oxidation ceramsite.

2. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The preparation method meets one or more of the following conditions: (1) The moisture content of the dried sludge powder is 1%-5%; (2) The particle size D50 of the dried sludge powder is 15-25 μm; (3) The dried sludge powder is obtained by dehydrating and crushing the raw sludge; (4) The solvent is one or more of deionized water, methanol, ethanol and isopropanol; (5) The ratio of the mass of the dried sludge powder to the volume of the solvent is 100 g: (70-80) mL.

3. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The binder is one or more of sodium carboxymethyl cellulose, sodium carboxymethyl starch, polyacrylic acid and polyacrylamide; And / or, the particle size of the spherical particles is 3-10 mm, preferably 3-5 mm.

4. The method for preparing catalytic oxidation ceramsite according to claim 3, characterized in that: When the binder is sodium carboxymethyl cellulose and / or sodium carboxymethyl starch, the mass ratio of the dry sludge powder to the binder is 100:(0.5-4); When the binder is polyacrylic acid and / or polyacrylamide, the mass ratio of the dry sludge powder to the binder is 1000:(0.5-4).

5. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The metal in the transition metal salt solution includes one or more of Fe, Mn and Co; and / or, the transition metal salt is one or more of metal citrate, metal acetate, metal acetylacetonate, metal chloride, metal nitrate and metal sulfate; Preferably, the transition metal salt solution is a ferric citrate solution; And / or, the concentration of the transition metal salt solution is 0.1-1M.

6. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The soaking time is 5-10 seconds; And / or, during the soaking, the volume of the transition metal salt solution can completely cover the pellets; The soaking preferably comprises the following steps: soaking the pellets in a 0.2M ferric citrate solution for 5-10 seconds.

7. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The spraying is to spray the transition metal salt solution on the surface of the pellets using a spray pot or a coating machine; and / or, during the spraying, the ratio of the mass of the pellet to the volume of the transition metal salt solution is 100 g: (1.5-3) mL; Preferably, the spraying comprises the following steps: using a spray pot, spraying 0.2M ferric citrate solution on the surface of the pellets, and the ratio of the mass of the pellets to the volume of the ferric citrate solution is preferably 100g:(1.5-3)mL.

8. The method for preparing catalytic oxidation ceramsite according to claim 1, characterized in that: The calcination temperature is 1000-1100°C; And / or, the calcination time is 1-4h.

9. Catalytic oxidation ceramsite obtained by the method for preparing catalytic oxidation ceramsite according to any one of claims 1 to 8.

10. Use of the catalytic oxidation ceramsite as claimed in claim 9 in sewage treatment.

Citation Information

Patent Citations

  • Preparation method and application of sludge-based ceramic catalyst

    CN109225187A

  • Ceramsite catalyst for sewage treatment as well as preparation method and application method thereof

    CN111468106A

  • Ceramsite catalyst based on activated sludge biomass fuel ash and preparation method and application thereof

    CN115337922A

  • Zero-valent iron ceramsite as well as preparation method and application thereof

    CN115724683A

  • Waste treatment

    US4872993A