Three-dimensional ordered hierarchical pore CuO / CeO2 catalyst constructed by template method and preparation method and application thereof

The three-dimensional orderly multi-stage porous CuO/CeO2 catalyst was constructed by the template method, which solved the problem of easy agglomeration of the catalyst at high temperatures, achieved efficient catalytic CO conversion at low temperatures, reduced costs, and was suitable for industrial production.

CN118892839APending Publication Date: 2024-11-05JIANGXI AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957430.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-05

Smart Images

  • Figure CN118892839A_ABST
    Figure CN118892839A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional ordered hierarchical pore CuO / CeO2 catalyst constructed by a template method as well as a preparation method and application of the three-dimensional ordered hierarchical pore CuO / CeO2 catalyst. The preparation method of the catalyst comprises the following steps: performing constant-temperature heating, stirring, water adding and cooling, ultrasonic treatment, high-speed centrifugation, water adding and recombination, water bath drying and the like on methyl methacrylate and potassium persulfate to obtain a three-dimensional ordered polymethyl methacrylate template agent; the CuO / CeO2 supported catalyst is prepared by further supporting CuO with an impregnation method, the content (mass ratio) of the active metal CuO in the CuO / CeO2 catalyst is 1.0%-20.0%, and the content of CeO2 is 80.0%-99.0%. The CuO / CeO2 catalyst is applied to a CO oxidation and hydrogen-rich oxidation catalytic system, and catalyst performance evaluation including CO conversion rate, O2 selectivity and the like is carried out in different temperature intervals. In addition, the metal carrier interaction (MSI) is regulated, the catalyst structure is optimized, and the catalytic activity is improved. The three-dimensional ordered hierarchical pore structure constructed by the scheme is beneficial to improving the low-temperature activity of the CuO / CeO2 catalyst, and provides a research basis and technology for CO oxidation and hydrogen-rich oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention relates to the field of three-dimensional ordered multi-level porous materials and chemical catalysis technology, specifically a three-dimensional ordered multi-level porous CuO / CeO2 catalyst constructed by a template method and its preparation method and application. Background Art

[0002] In proton exchange membrane fuel cells (PEMFCs), hydrogen, the main fuel, inevitably contains a small amount of CO. CO will combine with the Pt electrode of the PEMFC cell, occupy and inhibit the active sites of the hydrogen reaction, and poison the Pt electrode, thereby reducing the battery performance. In addition, in a confined and narrow space, CO is harmful to human life, health and safety. Therefore, eliminating CO through catalysis has important research value and strategic significance.

[0003] Using PMMA as a catalyst template not only increases the specific surface area of ​​the catalyst, but also can highly disperse active species and reduce agglomeration. The patent with publication number CN201911011392.0 involves a three-dimensional ordered macroporous oxygen-deficient cerium dioxide catalyst and its preparation method and application. The prepared catalyst is used for photothermal catalytic purification of typical atmospheric pollutants such as styrene, n-hexane and cyclohexane, but the invention is not used in combination with a supported catalyst. A precious metal catalyst for catalytic oxidation of CO and its preparation method disclosed in publication number CN114643065A, but because it uses precious metals as active species, the catalyst cost is high and is not suitable for industrial production. Through experiments, we found that the CuO / CeO2 catalyst constructed with PMMA as a template has better activity at lower temperatures, CO has been completely converted at 80°C, and PMMA as a template can regulate the three-dimensional ordered pore structure of CuO / CeO2, ranging from 140-350nm. Therefore, expanding the three-dimensional ordered multi-level pore structure of CuO / CeO2 catalyst with PMMA as template and applying it to CO catalytic conversion will help further explore the effects of high dispersion of active species and metal-support interaction on CO catalytic conversion.

[0004] Copper (Cu)-based catalysts tend to aggregate at high temperatures. By adding the template agent PMMA, the morphology of the catalyst is improved to form a three-dimensional ordered multi-level pore structure, and lowering the reaction temperature is an urgent problem to be solved. Therefore, it is necessary to regulate the morphology of active metal copper and test the activity in different temperature ranges. Exploring the morphology and structure of Cu-based catalysts for CO catalytic conversion is conducive to the further development of the reaction.

[0005] 1. Technical solution

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention discloses a three-dimensional ordered multi-level porous CuO / CeO2 catalyst constructed by a template method and a preparation method and application thereof. The catalyst is a mixed oxide of components with different mass fractions:

[0008] Metallic copper, consisting of copper (Cu) or its oxide (CuO) or a combination of the two, about 1-20%;

[0009] The catalyst carrier is mainly composed of cerium dioxide (CeO2), about 80-99%.

[0010] Further, copper (Cu) or its oxide (CuO) or a combination of the two, but not limited to copper nitrate monohydrate, copper nitrate trihydrate, cuprous chloride, copper oxide, copper acetate, copper sulfate, copper acetate and other inorganic salts are prepared as precursors;

[0011] The polymethyl methacrylate described in the present invention is used as a template agent and is produced by a constant temperature stirring polymerization process using purchased methyl methacrylate as a raw material;

[0012] Further, add 650 mL of deionized water (can be increased or decreased in proportion) into a 1000 mL three-necked flask and stir for 5-30 min under nitrogen protection;

[0013] Further, 30-70 mL of methyl methacrylate is added and stirred for 5-45 min;

[0014] Further, 0.1-0.5 g of potassium persulfate is added;

[0015] Further, 0.1-0.5 g of PVP dispersant was added, the reaction was stopped after 20-60 min, poured into cooling water, and cooled for 3-8 h;

[0016] Further, the cooled solution was subjected to high-speed centrifugation, the supernatant was discarded, and the solution was reconstituted with a small amount of deionized water. After being taken out, the solution was ultrasonicated for 10-30 minutes, poured into a small beaker, dried in a water bath at 80° C., and collected for later use.

[0017] The method for preparing the supported catalyst of the above-mentioned components in the present invention comprises the following steps:

[0018] S1: dispersing appropriate amounts of copper and cerium metal salt precursors in water and ethanol solutions;

[0019] S2: Pour an equal amount of PMMA into the above solution, and ensure that the PMMA is completely immersed;

[0020] S3: Further, seal with tin foil and let stand for 2-10 hours;

[0021] S4: Further, after filtering and drying the above catalyst, calcining it in a tubular furnace at 100-300° C. for 2 hours under a nitrogen atmosphere, and calcining it in a muffle furnace at 300-600° C. for 2 hours, to obtain the CuO / CeO2 catalyst.

[0022] The catalyst used in the present invention is a CO catalytic elimination reaction with a temperature range of 45-200°C and a space velocity of 1200-46000h -1 Under the conditions of , the catalyst is subjected to in-situ reduction treatment, the reaction gas (a mixture of hydrogen (under hydrogen-rich oxidation conditions), carbon monoxide, oxygen, and nitrogen) is introduced into a fixed bed reactor, and the product is detected by gas chromatography;

[0023] The results show that the three-dimensional ordered hierarchical CuO / CeO2 catalyst constructed by the template method exhibits good activity for CO catalytic conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope image of the template PMMA in the present invention.

[0025] Figure 2 This is a scanning electron microscope image of the catalyst of Example 1 of the present invention.

[0026] Figure 3 It is the Raman spectrum of the catalyst in Example 1-5 of the present invention. DETAILED DESCRIPTION

[0027] The present invention is described below by means of specific embodiments, but the present invention is not limited thereto.

[0028] The preparation methods and conditions used in the following examples are conventional methods unless otherwise specified; the reagents, gases, materials, etc. used in the following examples are all commercially available unless otherwise specified.

[0029] [Example 1]

[0030] (1) Preparation of PMMA:

[0031] Place 500mL of deionized water in a 1000mL three-necked flask, place the three-necked flask in an 85°C oil bath, stir at 85°C for 25min under a nitrogen atmosphere, add 50ml of methyl methacrylate, stir for 20min under a nitrogen atmosphere, add 0.18g of potassium persulfate, react for 35min, pour the reaction solution in the three-necked flask into 1000mL of pre-cooled deionized water and put it in an ice bag for cooling for 8 hours, centrifuge the cooled solution at a speed of 5000r / min for 30min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 30min, transfer the ultrasonicated solution into a 10mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0032] (2) Preparation of CuO / CeO2 catalyst

[0033] Weigh 1.8248g of cerium acetate and 0.01g of copper oxide, dissolve them in 18mL of ethanol-water solution mixed in equal proportions, add 0.5g of dispersant PAN, stir for 30min, and then put the PMMA obtained in the above step (1) in a ratio of 1:1. The PMMA needs to be completely immersed in the solution for 2 hours, and the excess solution is filtered out with a funnel until the surface is slightly dry, and then vacuum dried at 80℃ overnight. In an argon atmosphere, the dried material is placed in a tube furnace at 1℃ / min, 200℃, 2h, and then placed in a muffle furnace at 2℃ / min, 500℃, 2h. Finally, a three-dimensional ordered porous 1wt% CuO / CeO2 catalyst 1 is obtained.

[0034] (3) Catalyst activity test

[0035] The catalyst obtained in (2) was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced. The space velocity was set to 9000 h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0036] [Example 2]

[0037] (1) Preparation of PMMA:

[0038] Place 700mL of deionized water in a 1000mL three-necked flask, place the three-necked flask in an 82°C oil bath, stir at 82°C for 10min under a nitrogen atmosphere, add 60ml of methyl methacrylate, stir for 15min under a nitrogen atmosphere, add 0.23g of potassium persulfate, react for 40min, pour the reaction solution in the three-necked flask into 1000mL of pre-cooled deionized water and put it in an ice bag for cooling for 6 hours, centrifuge the cooled solution at a high speed of 5000r / min for 30min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 15min, transfer the ultrasonicated solution into a 10mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0039] (2) Preparation of CuO / CeO2 catalyst

[0040] Weigh 0.95g of cerium oxide and 0.3020g of copper nitrate trihydrate, dissolve them in 20mL of ethanol-water solution mixed in equal proportion, add 0.2g of dispersant PVP, stir for 18min, and then put PMMA obtained in the above step (1) in a ratio of 1:1. The PMMA needs to be completely immersed in the solution for 5 hours, and the excess solution is filtered out with a funnel until the surface is slightly dry, and then vacuum dried at 80℃ overnight. In an argon atmosphere, the dried material is placed in a tube furnace at 1℃ / min, 300℃, 2h, and then placed in a muffle furnace at 2℃ / min, 500℃, 2h. Finally, a three-dimensional ordered porous 5wt% CuO / CeO2 catalyst 2 is obtained.

[0041] (3) Catalyst activity test

[0042] The catalyst obtained in (2) was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced. The space velocity was set to 20000h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0043] [Example 3]

[0044] (1) Preparation of PMMA:

[0045] Place 650mL of deionized water in a 1000mL three-necked flask, place the three-necked flask in an 80°C oil bath, stir at 80°C for 30min under a nitrogen atmosphere, add 70ml of methyl methacrylate, stir for 15min under a nitrogen atmosphere, add 0.25g of potassium persulfate, react for 43min, pour the reaction solution in the three-necked flask into 1000mL of pre-cooled deionized water and put it in an ice bag for cooling for 8 hours, centrifuge the cooled solution at a speed of 5000r / min for 30min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 30min, transfer the ultrasonicated solution into a 10mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0046] (2) Preparation of CuO / CeO2 catalyst

[0047] Weigh 4.5400g of cerium nitrate hexahydrate and 0.6040g of copper nitrate trihydrate, dissolve them in 16mL of ethanol-water solution mixed in equal proportion, add 0.2g of dispersant PAN, stir for 20min, and then put PMMA obtained in the above step (1) in a ratio of 1:1. The PMMA needs to be completely immersed in the solution for 6 hours, and the excess solution is filtered out with a funnel until the surface is slightly dry, and then vacuum dried at 80℃ overnight. In an argon atmosphere, the dried material is placed in a tube furnace at 1℃ / min, 300℃, 2h, and then placed in a muffle furnace at 2℃ / min, 500℃, 2h. Finally, a three-dimensional ordered porous 10wt% CuO / CeO2 catalyst 3 is obtained.

[0048] (3) Catalyst activity test

[0049] The catalyst obtained in (2) was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced. The space velocity was set to 35000 h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0050] [Example 4]

[0051] (1) Preparation of PMMA:

[0052] Place 750mL of deionized water in a 1000mL three-necked flask, place the three-necked flask in a 92°C oil bath, stir at 92°C for 30min under a nitrogen atmosphere, add 70ml of methyl methacrylate, stir for 25min under a nitrogen atmosphere, add 0.25g of potassium persulfate, react for 28min, pour the reaction solution in the three-necked flask into 1000mL of pre-cooled deionized water and put it in an ice bag for cooling for 10 hours, centrifuge the cooled solution at a speed of 5000r / min for 30min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 30min, transfer the ultrasonicated solution into a 10mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0053] (2) Preparation of CuO / CeO2 catalyst

[0054] 1.5667g of cerium acetate and 0.9058g of copper nitrate trihydrate were dissolved in 20mL of ethanol-water solution mixed in equal proportions, 0.1g of citric acid was added as a dispersant, and after stirring for 15min, the PMMA obtained in the above step (1) was added in a 1:1 ratio. The PMMA was completely immersed in the solution for 5 hours, and the excess solution was filtered out with a funnel until the surface was slightly dry, and then vacuum dried at 80°C overnight. In an argon atmosphere, the dried material was placed in a tube furnace at 1°C / min, 300°C, 2h, and then placed in a muffle furnace at 2°C / min, 480°C, 2h. Finally, a three-dimensional ordered porous 15wt% CuO / CeO2 catalyst 4 was obtained.

[0055] (3) Catalyst activity test

[0056] The catalyst obtained in (2) was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced. The space velocity was set to 22000h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0057] [Example 5]

[0058] (1) Preparation of PMMA:

[0059] Place 550 mL of deionized water in a 1000 mL three-necked flask, place the three-necked flask in an 85°C oil bath, stir at 85°C for 30 min under a nitrogen atmosphere, add 45 ml of methyl methacrylate, stir for 20 minutes under a nitrogen atmosphere, add 0.17 g of potassium persulfate, react for 37 min, pour the reaction solution in the three-necked flask into 1000 mL of pre-cooled deionized water and put it in an ice bag for cooling for 10 hours, centrifuge the cooled solution at a high speed of 5000 r / min for 30 min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000 mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 30 min, transfer the ultrasonicated solution into a 10 mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0060] (2) Preparation of CuO / CeO2 catalyst

[0061] Weigh 4.0356g of cerium nitrate hexahydrate and 0.4491g of copper acetate, dissolve them in 18mL of ethanol-water solution mixed in equal proportions, add 0.4g of citric acid as a dispersant, stir for 35min, and then put the PMMA obtained in the above step (1) in a 1:1 ratio. The PMMA needs to be completely immersed in the solution for 2 hours, and the excess solution is filtered out with a funnel until the surface is slightly dry, and then vacuum dried at 80℃ overnight. In an argon atmosphere, the dried material is placed in a tube furnace at 1℃ / min, 300℃, 2h, and then placed in a muffle furnace at 2℃ / min, 480℃, 2h. Finally, a three-dimensional ordered porous 20wt% CuO / CeO2 catalyst 5 is obtained.

[0062] (3) Catalyst activity test

[0063] The catalyst obtained in (2) was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced. The space velocity was set to 3900 h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0064] [Example 6]

[0065] (1) Preparation of PMMA:

[0066] Place 650mL of deionized water in a 1000mL three-necked flask, place the three-necked flask in an 80°C oil bath, stir at 80°C for 30min under a nitrogen atmosphere, add 70ml of methyl methacrylate, stir for 15min under a nitrogen atmosphere, add 0.25g of potassium persulfate, react for 35min, pour the reaction solution in the three-necked flask into 1000mL of pre-cooled deionized water and put it in an ice bag for cooling for 8 hours, centrifuge the cooled solution at a speed of 5000r / min for 30min, discard the supernatant, reconstitute with an equal volume of deionized water, and place in a 2000mL beaker. After all the reconstitution is completed, ultrasonicate the resulting solution for 30min, transfer the ultrasonicated solution into a 10mL small beaker, evaporate to dryness in an 80°C water bath, and collect for use.

[0067] (2) Preparation of CuO / CeO2 catalyst

[0068] Weigh 1.6589g of cerium acetate and 0.0794g of cuprous chloride, add citric acid in the ratio of 2:1 of the total amount of copper-cerium precursor: citric acid, dissolve them in 10mL of ethanol-water solution mixed in equal proportions, stir for 15min, and then add PMMA obtained in the above step (1) in a ratio of 1:1. The PMMA needs to be completely immersed in the solution for 2 hours, and the excess solution is filtered out with a funnel until the surface is slightly dry, and then vacuum dried at 80℃ overnight. In an argon atmosphere, the dried material is placed in a tube furnace at 1℃ / min, 300℃, 2h, and then placed in a muffle furnace at 2℃ / min, 600℃, 2h. Finally, a three-dimensional ordered porous 10wt% CuO / CeO2 catalyst 6 is obtained.

[0069] (3) Catalyst activity test

[0070] The catalyst obtained in (2) above was passed through a fixed bed catalyst evaluation device, and CO, O2, H2 (rich hydrogen oxidase) and N2 in appropriate proportions were introduced, and the space velocity was set to 30000h -1 , and test the composition and proportion of the exhaust gas during the programmed temperature rise stage.

[0071] Table 1: Design parameters of Examples 1-6

[0072]

[0073]

[0074]

Claims

1. A three-dimensional ordered multi-level porous CuO / CeO2 catalyst constructed by a template method and its preparation method and application, comprising the following features: in, The template is based on polymethyl methacrylate (PMMA) formed by the polymerization of methyl methacrylate (MMA); and as a template, the pore size and structure of the PMMA template are regulated, and a three-dimensional ordered multi-level porous CuO / CeO2 catalyst is prepared; CeO2 is used as a carrier of the catalyst, with a mass proportion of 80.0% to 99.0%; CuO is used as an active metal, with a mass proportion of 1.0% to 20.0%.

2. The PMMA template according to claim 1, characterized in that: A PMMA template with an ordered structure is obtained by using MMA as a precursor through anaerobic polymerization, centrifugal reorganization, water bath drying and other steps.

3. The method for controlling PMMA pore size and structure according to claim 1, characterized in that: By adjusting the reaction time, polymerization temperature and dispersant, etc., PMMA templates with different pore sizes and structures can be obtained.

4. The dispersant according to claim 3, characterized in that: Including but not limited to polyvinyl pyrrolidone PVP, polyacrylonitrile PAN and citric acid.

5. The method for preparing the three-dimensional ordered multi-level porous CuO / CeO2 catalyst according to claim 1 comprises the following steps: The catalyst was prepared by a one-step impregnation method, in which the catalyst precursor and a mixed solution of ethanol and water were infiltrated into PMMA with different pore sizes and structures. The three-dimensional ordered hierarchical CuO / CeO2 catalyst was then obtained through filtration, drying, carbonization and calcination.

6. The catalyst precursor according to claim 5, characterized in that: The precursors include but are not limited to copper nitrate monohydrate, copper nitrate trihydrate, cuprous chloride, cupric oxide, cupric acetate, copper sulfate, copper acetate and other inorganic salt precursors; the CeO2 precursors include but are not limited to cerium nitrate hexahydrate, cerium acetate, cerium oxide and other inorganic salt precursors.

7. The mixed solution of ethanol and water according to claim 5, characterized in that: The solvent includes but is not limited to water, ethanol and mixed solutions thereof.

8. The use of a three-dimensional ordered multi-level porous CuO / CeO2 catalyst according to claim 1, characterized in that: Used in CO oxidation and CO hydrogen-enriched oxidation reaction systems. Use a fixed bed evaluation device, introduce appropriate proportions of CO, O2 (H2 is required for hydrogen-enriched oxidation) and diluent gas N2, and test at different temperature ranges (45-200°C).