Preparation method and application of multi-metal oxide containing hindered Lewis acid-base pair
By introducing transition metal atoms into metal oxides to form a hindered Lewis acid-base pair polymetal oxide catalyst, the problem that oxygen is difficult to activate sulfides is solved, and high-efficiency deep desulfurization in oxidized diesel is achieved. The catalyst has high activity and good Cyclic stability.
Patent Information
- Application Number
- CN202410928797.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
In the existing oxidative and desulfurization technology, oxygen is difficult to activate sulfides, and heterogeneous catalysts such as iron oxides are rarely used in this field, resulting in low desulfurization efficiency. High-efficiency catalysts are needed to assist in the oxidative and desulfurization reaction.
Transition metal atoms are introduced into metal oxides through atom doping strategy to form a hindered Lewis acid-base pair, and independent Lewis acid sites adsorb aromatic organic sulfur, and Lewis base sites activate molecular oxygen, and synergistically catalyzed oxidation and desulfurization. The specific method includes reacting a transition metal doping source with a coordination metal source in a solvent to form a catalyst precursor, and calcining in an atmosphere to obtain a polymetal oxide catalyst containing a hindered Lewis acid-base pair.
It has achieved efficient removal of aromatic sulfur-containing compounds in oxidized diesel, the catalyst has high activity and good cycle stability, and can be deeply desulfurized under mild conditions without by-products.
Smart Images

Figure CN118892842A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional material preparation, and in particular relates to a multi-metal oxide catalyst containing a hindered Lewis acid-base pair, and further provides a preparation method of the catalyst and an application of the catalyst in catalytic oxidation diesel desulfurization. Background Art
[0002] In recent years, with the rapid development of the automobile industry, harmful gases such as SOx produced by fuel combustion can cause acid rain, environmental pollution, and threaten human health. Therefore, in order to reduce the harm of sulfides, governments around the world strictly limit the sulfide content in fuel (≤10ppm). At present, the most widely used desulfurization technology in industry is hydrodesulfurization (HDS), but because the thiophene sulfides in fuel are more complex in structure than aliphatic sulfides, the removal conditions are harsh, which leads to an increase in production costs for enterprises. Therefore, it is necessary to find new desulfurization technologies to assist in achieving deep desulfurization of fuel. Oxidative desulfurization technology is considered to be one of the desulfurization methods with development prospects due to its mild reaction conditions and low energy consumption.
[0003] In the oxidative desulfurization process with oxygen as the oxidant, since the oxygen molecule is in an inert triplet ground state, it is difficult to activate the sulfide, so it is necessary to design an efficient catalyst to jointly activate molecular oxygen and sulfur-containing substrates. Transition metal oxides have high activity in the cleavage and conversion of CS bonds in aromatic sulfur-containing compounds, so they are often used in oxidative desulfurization. However, heterogeneous catalysts based on iron oxide have a stable electronic structure and are rarely reported in the field of oxidative desulfurization. Therefore, in order to further improve the application of metal-based catalysts in oxidative desulfurization, they need to be modified.
[0004] Atomic doping is one of the most effective methods to adjust the electronic structure of catalysts. By changing the surface acidity and alkalinity of metals through the synergistic effect between the main body and the doped metal atoms, weakly alkaline aromatic sulfur-containing compounds can be effectively adsorbed. At the same time, it was found during the research process that hindered Lewis acid-base pairs (FLP) are a type of Lewis acid-base pairs with special reactivity, which can make Lewis acids and Lewis bases exist independently as electron pair acceptors and donors to activate small molecules.
[0005] However, no research has been reported on the activation of molecular oxygen desulfurization by a host multi-metal catalyst containing a hindered Lewis acid-base pair in the current study. Therefore, it is necessary to report a new technical solution. Summary of the invention
[0006] In view of the problems existing in existing research and technology, the purpose of the present invention is to provide a multi-metal oxide containing a hindered Lewis acid-base pair for catalytic oxidation diesel desulfurization reaction. The present invention adopts an atomic doping strategy to dope transition metal atoms into the metal oxide lattice, wherein the metal site adjacent to the doped atom serves as a Lewis acid site, and the doped atom adjacent to the oxygen vacancy serves as a Lewis base site, so as to obtain a multi-metal oxide catalyst containing a hindered Lewis acid-base pair. The independent Lewis acid sites in the hindered Lewis acid-base pair structure adsorb and activate aromatic organic sulfur, while the independent Lewis base sites in the structure effectively activate molecular oxygen, forming a synergistic catalytic environment and improving the performance of oxidative desulfurization.
[0007] Another technical problem to be solved by the present invention is to provide a preparation process of the above-mentioned multi-metal oxide catalyst containing a hindered Lewis acid-base pair.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a multi-metal oxide containing a hindered Lewis acid-base pair comprises the following steps:
[0010] (1) dissolving a transition metal doping source and a coordination metal source in a mixed solution of N,N-dimethylformamide and ethylene glycol, stirring the mixture until no obvious particles are present, adding a certain amount of 1,3,5-benzenetricarboxylic acid, and stirring the mixture thoroughly to form a uniform mixed solution;
[0011] (2) adding the mixed solution prepared in step (1) into a polytetrafluoroethylene liner, performing a solvent thermal reaction at a certain temperature, cooling to room temperature after the reaction is completed, centrifuging, washing with anhydrous ethanol, and drying to obtain a catalyst precursor;
[0012] (3) placing the precursor sample obtained in step (2) in a tubular electric furnace and heating it to a calcination temperature in a gas atmosphere at a certain heating rate to obtain a multi-metal oxide catalyst containing a hindered Lewis acid-base pair.
[0013] In step (1), the transition metal doping source is one or more of ammonium molybdate tetrahydrate, ammonium molybdate, ammonium tungstate, ammonium metavanadate or titanate, preferably ammonium molybdate tetrahydrate.
[0014] The coordination metal source is one of ferric chloride hexahydrate, ferric nitrate nonahydrate, chromium nitrate, aluminum nitrate nonahydrate, and vanadium trichloride; preferably ferric chloride hexahydrate.
[0015] Wherein, the molar ratio of metal ions in the transition metal doping source and the coordination metal source is 0.5:10 to 3:10;
[0016] In the mixed solution of N,N-dimethylformamide and ethylene glycol, the volume ratio of N,N-dimethylformamide to ethylene glycol is 1:1;
[0017] The molar ratio of 1,3,5-benzenetricarboxylic acid to the coordination metal source is 1.5 to 2:1.
[0018] In step (2), the temperature of the solvent thermal reaction is 100-140° C. and the time is 6-18 hours.
[0019] In step (3), the heating rate is 5-10°C / min, the calcination temperature is 400-800°C, and the calcination time is 1-6h. The gas atmosphere is: air, oxygen, or a mixed gas containing a certain oxygen component.
[0020] The multi-metal oxide catalyst containing hindered Lewis acid-base pairs prepared by the invention has a powdery solid appearance and is immiscible with liquids such as water, ethanol, acetonitrile, gasoline and diesel, and is an environmentally friendly catalyst.
[0021] In addition, the multi-metal oxide containing hindered Lewis acid-base pairs prepared by the present invention can be used to remove aromatic sulfur-containing compounds in catalytic oxidation diesel. The specific steps are as follows:
[0022] The multimetal oxide containing hindered Lewis acid-base pairs prepared by the present invention is added to simulated diesel containing aromatic sulfides, oxygen is introduced, and the mixture is stirred in a constant temperature oil bath at a temperature of 110-130° C. and a stirring speed of 600 rpm for reaction, and the upper oil phase is taken for testing the sulfur content in the oil product. After the reaction is complete, the oil phase and the catalyst phase are centrifugally separated, washed, and dried for recycling.
[0023] The simulated diesel containing aromatic sulfides is prepared by dissolving dibenzothiophene (DBT), 4-methyldibenzothiophene (4-MDBT), and 4,6-dimethyldibenzothiophene (4,6-DMDBT) in dodecane, with a sulfur content of 200 mg kg -1 .
[0024] In the above desulfurization step, the ratio of the multi-metal oxide containing the hindered Lewis acid-base pair to the simulated diesel is 5-20 mg: 20 mL;
[0025] The oxidant is oxygen with a flow rate of 80-120 mL / min.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The invention utilizes an atomic doping strategy to dope transition metals such as molybdenum, tungsten, vanadium, and titanium into the lattices of metal iron oxide, zirconium oxide, vanadium oxide, and aluminum oxide, and adjusts the electronic structure of the catalyst so that abundant Lewis acid sites are generated in the metal oxide structure. The doped atoms adjacent to the oxygen vacancies serve as Lewis base sites, and due to the steric hindrance effect, hindered Lewis acid-base pairs are formed. The Lewis acid-base pairs that exist independently in the catalyst can achieve adsorption and activation of oxygen molecules and sulfur-containing substrate molecules, thereby exhibiting excellent catalytic performance in diesel oxidative desulfurization. However, no previous research reports have reported the application of hindered Lewis acid-base pairs in oxidative desulfurization.
[0028] (2) The multi-metal oxide catalyst containing a hindered Lewis acid-base pair of the present invention has the characteristics of high activity and easy separation of a heterogeneous catalyst, and its activity has good cycle stability, and can achieve deep desulfurization. At the same time, no other by-products are generated during the desulfurization process.
[0029] (3) The multimetal oxide catalyst containing a hindered Lewis acid-base pair of the present invention adopts a "ship in a bottle" strategy to make the transition metal doping atoms highly dispersed in the catalyst. After the atoms are doped, the surface chemical properties and surface acid-base distribution sites of the oxide catalyst itself are changed, providing new insights into improving the activity of heterogeneous catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The UV-visible diffuse reflectance spectra of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention are shown;
[0031] Figure 2 The electron spin resonance spectrum of a molybdenum-doped iron oxide catalyst containing a hindered Lewis acid-base pair provided in Example 1 of the present invention;
[0032] Figure 3 This is a graph showing the desulfurization performance of the catalysts synthesized in Example 1, Comparative Example 2 and Comparative Example 3.
[0033] Figure 4 It is a graph showing the desulfurization performance of the catalyst synthesized in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, a clear and complete description is given below in combination with the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are partial embodiments of the present invention, rather than all examples.
[0035] Embodiment 1:
[0036] (1) Weigh 0.0698 g of ammonium molybdate tetrahydrate and 0.1557 g of ferric chloride hexahydrate and dissolve them in a mixed solution of 15 mL of N,N-dimethylformamide and 15 mL of ethylene glycol. Stir well and then add 0.2298 g of 1,3,5-benzenetricarboxylic acid. Stir thoroughly to form a uniform mixed solution.
[0037] (2) The mixed solution was added to a polytetrafluoroethylene liner and subjected to a solvothermal reaction at 120° C. for 12 hours. The obtained sample was in a gel state, which was centrifuged, washed with anhydrous ethanol, and dried to obtain a precursor of a molybdenum-doped iron oxide catalyst.
[0038] (3) The precursor is then calcined at 700° C. at a heating rate of 10° C. / min in an air atmosphere for 3 hours to obtain a molybdenum-doped iron oxide catalyst containing a hindered Lewis acid-base pair.
[0039] Its hindered Lewis acid-base pair is constructed by using the iron atom adjacent to the molybdenum atom as the Lewis acid site and the molybdenum atom adjacent to the oxygen vacancy as the Lewis base site. Figure 1 The absorption peak position of the UV-visible diffuse reflectance spectrum is red-shifted. Figure 2 Electron spin resonance spectroscopy revealed oxygen vacancies in the catalyst.
[0040] Catalytic oxidation desulfurization of oil products:
[0041] 20 mg of catalyst was mixed with 20 mL of 200 mg kg -1 The mixture was mixed with DBT and oxygen (120 mL / min) was introduced, and the mixture was stirred in an oil bath at 600 rpm and reacted at 120°C. Samples were taken at regular intervals and the sulfur content in the simulated oil was detected by gas chromatography. The results are shown in the attached figure. Figure 3 and attached Figure 4 As shown, the desulfurization rate of the catalyst corresponding to Example 1 can reach 100% within 3 hours.
[0042] Embodiment 2:
[0043] (1) Weigh ammonium tungstate and chromium nitrate according to the metal source molar ratio of 2:10, dissolve in a mixed solution of 15 mL N,N-dimethylformamide and 15 mL ethylene glycol, stir evenly, then add 0.2298 g 1,3,5-benzenetricarboxylic acid, and stir thoroughly to form a uniform mixed solution.
[0044] (2) The mixed solution was added to a polytetrafluoroethylene liner and subjected to a solvothermal reaction at 120° C. for 12 hours. The obtained sample was in a gel state, which was centrifuged, washed with anhydrous ethanol, and dried to obtain a precursor of a tungsten-doped chromium oxide catalyst.
[0045] (3) The precursor is then calcined at 700° C. at a heating rate of 10° C. / min in an air atmosphere for 3 hours to obtain a tungsten-doped chromium oxide catalyst containing a hindered Lewis acid-base pair.
[0046] Example 3
[0047] (1) Ammonium vanadate and aluminum nitrate were weighed in a metal source molar ratio of 3:10, dissolved in a mixed solution of 15 mL of N,N-dimethylformamide and 15 mL of ethylene glycol, stirred evenly, and then 0.2298 g of 1,3,5-benzenetricarboxylic acid was added and stirred thoroughly to form a uniform mixed solution.
[0048] (2) The mixed solution was added to a polytetrafluoroethylene liner and subjected to a solvothermal reaction at 120° C. for 12 hours. The obtained sample was in a gel state, which was centrifuged, washed with anhydrous ethanol, and dried to obtain a precursor of a vanadium-doped alumina catalyst.
[0049] (3) The precursor is then calcined at 700° C. at a heating rate of 10° C. / min in an air atmosphere for 3 hours to obtain a vanadium-doped alumina catalyst containing a hindered Lewis acid-base pair.
[0050] Comparative Example 1
[0051] (1) Weigh 0.0698 g of ammonium molybdate tetrahydrate and 0.1557 g of ferric chloride hexahydrate and dissolve them in a mixed solution of 15 mL of N,N-dimethylformamide and 15 mL of ethylene glycol, and stir to form a uniform mixed solution.
[0052] (2) The mixed solution was added to a polytetrafluoroethylene liner and subjected to a solvothermal reaction at 120° C. for 12 hours. The obtained sample was in a gel state, which was centrifuged, washed with anhydrous ethanol, and dried to obtain a mixture precursor.
[0053] (3) The precursor is then calcined at 700° C. for 3 hours at a heating rate of 10° C. / min in an air atmosphere to obtain a molybdenum-iron bimetallic oxide catalyst with a low Lewis acid-base matching degree.
[0054] Catalytic oxidation desulfurization of oil products:
[0055] 20 mg of catalyst was mixed with 20 mL of 200 mg kg -1 The mixture was mixed with DBT and oxygen (120 mL / min) was introduced, and the mixture was stirred in an oil bath at 600 rpm and reacted at 120°C. Samples were taken at regular intervals and the sulfur content in the simulated oil was detected by gas chromatography. The results are shown in the attached figure. Figure 4After 3 hours of reaction, the desulfurization activity of the catalyst obtained in Comparative Example 1 was still in the latent period, and the desulfurization rate was less than 20%; after 7 hours of reaction, the desulfurization rate reached 88.0%; after 8 hours of reaction, the desulfurization rate reached 100%.
[0056] The desulfurization performance of this comparative example is as follows: adding 1,3,5-benzenetricarboxylic acid to the precursor is conducive to the formation of a MOF coating structure, and its abundant pores are more conducive to the dispersion of the doped metal source. It is easy to construct a hindered Lewis acid-base pair with suitable acidity and alkalinity during the calcination process, which is beneficial to the desulfurization performance.
[0057] Comparative Example 2
[0058] 0.1557 g of ferric chloride hexahydrate was dissolved in a mixed solution of 15 mL of N,N-dimethylformamide and 15 mL of ethylene glycol, and 0.2298 g of 1,3,5-benzenetricarboxylic acid was added and stirred to form a uniform mixed solution. Further, the mixed solution was subjected to a solvothermal reaction at 120 ° C for 12 hours, and the obtained sample was centrifuged, washed with anhydrous ethanol, and dried to obtain the precursor MIL-100 (Fe). The precursor was calcined at 700 ° C for 3 hours at 10 ° C / min in an air atmosphere to obtain a Fe2O3 catalyst.
[0059] 20 mg of iron oxide catalyst was mixed with 20 mL of DBT containing 200 mg kg-1, and oxygen (120 mL / min) was introduced. The mixture was stirred in an oil bath at 600 rpm and reacted at 120°C for 4 hours. Samples were taken at regular intervals and the sulfur content in the simulated oil was detected by gas chromatography. The desulfurization performance is shown in the attached figure. Figure 3 As shown, under the reaction conditions, the DBT removal rate of Fe2O3 catalyst was still less than 10% after 4 hours of reaction.
[0060] Comparative Example 3
[0061] Ferric molybdate was synthesized by coprecipitation method. First, ferric nitrate was dissolved in distilled water for later use, and then dropped into the prepared pre-acidified (pH=2, nitric acid) ammonium molybdate solution, and the prepared solution was reacted at 80°C for 3 hours, filtered (without washing and drying), and calcined at 700°C for 3 hours to obtain the ferric molybdate catalyst.
[0062] 20 mg of iron molybdate catalyst was mixed with 20 mL of DBT containing 200 mg kg-1, and oxygen (120 mL / min) was introduced. The mixture was stirred in an oil bath at 600 rpm and reacted at 120°C for 4 hours. Samples were taken at regular intervals and the sulfur content in the simulated oil was detected by gas chromatography. The desulfurization performance is shown in the attached figure. Figure 3 As shown, under the reaction conditions, the removal rate of DBT by Fe2O3 catalyst was less than 10% after 4 hours of reaction.
[0063] Various modifications to these examples will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.
Claims
1. A method for preparing a multi-metal oxide containing a hindered Lewis acid-base pair, characterized in that: The following steps are involved: (1) dissolving a transition metal doping source and a coordination metal source in a mixed solution of N,N-dimethylformamide and ethylene glycol, stirring the mixture until no obvious particles are present, adding a certain amount of 1,3,5-benzenetricarboxylic acid, and stirring the mixture thoroughly to form a uniform mixed solution; (2) adding the mixed solution prepared in step (1) into a polytetrafluoroethylene liner, performing a solvent thermal reaction at a certain temperature, cooling to room temperature after the reaction is completed, centrifuging, washing with anhydrous ethanol, and drying to obtain a catalyst precursor; (3) placing the precursor sample obtained in step (2) in a tubular electric furnace and heating it to a calcination temperature in a gas atmosphere at a certain heating rate to obtain a multi-metal oxide catalyst containing a hindered Lewis acid-base pair.
2. The preparation method according to claim 1, characterized in that In step (1), the transition metal doping source is one or more of ammonium molybdate tetrahydrate, ammonium molybdate, ammonium tungstate, ammonium metavanadate or titanate; the coordination metal source is one of ferric chloride hexahydrate, ferric nitrate nonahydrate, chromium nitrate, aluminum nitrate nonahydrate, and vanadium trichloride.
3. The preparation method according to claim 2, characterized in that: In step (1), the transition metal doping source is ammonium molybdate tetrahydrate, and the coordination metal source is ferric chloride hexahydrate.
4. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of metal ions in the transition metal doping source and the coordination metal source is 0.5:10 to 3:
10.
5. The preparation method according to claim 1, characterized in that: In step (1), in the mixed solution of N,N-dimethylformamide and ethylene glycol, the volume ratio of N,N-dimethylformamide to ethylene glycol is 1:
1.
6. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of 1,3,5-benzenetricarboxylic acid to the coordination metal source is 1.5 to 2:
1.
7. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the solvent thermal reaction is 100-140° C. and the time is 6-18 hours.
8. The preparation method according to claim 1, characterized in that: In step (3), the heating rate is 5-10°C / min, the calcination temperature is 400-800°C, and the calcination time is 1-6h; the gas atmosphere is: air, oxygen, or a mixed gas containing a certain oxygen component.
9. A multimetal oxide containing a hindered Lewis acid-base pair, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8, has a powdery solid appearance, and is immiscible with water, ethanol, acetonitrile, gasoline and diesel.
10. Use of the multimetal oxide containing hindered Lewis acid-base pairs according to claim 9 for catalytic oxidation of aromatic sulfur-containing compounds in diesel.
Citation Information
Patent Citations
High-efficiency hydrogen evolution catalyst and preparation method thereof
CN110433835A
Transition metal doped nickel molybdate catalyst as well as preparation method and application thereof
CN114768817A
Vanadium-cerium-based composite oxide denitration catalyst as well as preparation method and application thereof
CN115445603A
Method for preparing 1, 5-pentanediol based on efficient catalysis of M-M 'Ox non-noble metal catalyst
CN116903440A
Titanium-dioxide-based double-layer hollow material, preparation method thereof, and application thereof in photocatalytic treatment of hydrogen sulfide
US20180179079A1
Cited By
Fe / Ni co-doped W18O49 oxidative desulfurization catalyst as well as preparation method and application thereof