Iron-based supported low-temperature section denitration catalyst suitable for biomass combustion flue gas, preparation method and application
By using iron-based supported low-temperature-stage denitrification catalysts prepared with materials such as iron oxide and lanthanum manganate, the problem of poor catalytic effect of vanadium-based catalysts in the low-temperature segment is solved, and efficient nitrogen oxide removal and environmentally friendly smoke purification effects are achieved.
Patent Information
- Application Number
- CN202410943067.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, vanadium-based catalysts have poor catalytic effects in the low-temperature stage, and the active temperature window is narrow, making it difficult to effectively remove nitrogen oxides in the combustion flue gas of biomass.
Iron-based supported low-temperature denitrition catalysts using iron oxide as the support, lanthanum manganate as the active ingredient, and citric acid or oxalic acid as the complexing agent, improve the activity and stability of the catalyst through a specific preparation process, and is suitable for biomass combustion smoke. Denitrification of gas.
It achieves efficient nitrogen oxide removal rate in low-temperature stages, and the catalyst process is simple and low-cost. It is suitable for thermal power plants, industrial kilns and other fields, and the recycling of waste catalysts will not cause secondary pollution.
Smart Images

Figure CN118892845A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flue gas denitration catalysts, and in particular relates to an iron-based loaded low-temperature denitration catalyst suitable for biomass combustion flue gas, a preparation method and an application thereof. Background Art
[0002] Nitrogen oxides are one of the main gaseous pollutants in the atmosphere, which can have a serious impact on human health and the environment. Nitrogen oxides can cause harm to human lungs, reduce human resistance and cause respiratory diseases; nitrogen oxides are prone to a series of chemical reactions with volatile organic compounds (VOCs), causing a series of major environmental problems such as haze, acid rain and photochemical smog. Nitrogen oxides mainly include N2O, NO2, NO and N2O5, among which the nitrogen oxides that pollute the atmosphere are mainly NO2 and NO. In recent years, the emission control standards of nitrogen oxides and the technology for preventing and controlling nitrogen oxides remain the top priority of environmental governance.
[0003] Biomass energy is the fourth largest energy source after coal, oil and natural gas, and occupies an important position in the entire energy system. The use of biomass energy can effectively reduce carbon emissions, but due to the high content of nitrogen in biomass fuel, it produces more nitrogen oxides during the combustion process. With the popularization and application of large-scale biomass boilers, the NOx emission problem of biomass combustion flue gas has received more and more attention. Flue gas denitrification technology mainly includes post-denitrification treatment of flue gas and combustion process control, while selective catalytic reduction technology (SCR) is the most widely used and mature denitrification technology at home and abroad. The basic principle of the SCR method is to use reducing gas (such as NH3) as a reducing agent within a suitable temperature range to selectively react with nitrogen oxides under catalysis to generate non-toxic N2 and H2O.
[0004] At present, vanadium-based catalysts are widely used in the field of industrial denitrification. They have the advantages of excellent low-temperature activity and resistance to SO2 poisoning. They are one of the industrial catalysts widely studied by many scholars. However, due to the toxicity of V2O5, the oxidizing property of SO2 and the low selectivity to N2, vanadium-based catalysts are subject to certain restrictions in industrial applications. In the SCR reactor layout, the reactor in the low-temperature and low-dust system is placed after the desulfurization system and the dust removal system. In this layout, the catalyst is not easily poisoned, but this requires a low reaction temperature, usually 200°C or even lower. Therefore, the development of a catalyst with a wide high-activity temperature window and a high catalytic effect in the low-temperature section is the key to solving the problem of catalyst defects in denitrification technology. Summary of the invention
[0005] In view of the technical problems that the existing alum-based catalysts have a narrow active temperature window and a poor catalytic effect in the low-temperature stage, the present invention proposes an iron-based loaded low-temperature stage denitrification catalyst suitable for biomass combustion flue gas, a preparation method and an application. The catalyst of the present invention is a non-toxic and environmentally friendly loaded iron-based low-temperature stage denitrification catalyst with a simple production process, low cost, no addition of harmful substances, and no secondary pollution when the waste catalyst is recycled. It has an outstanding effect in SCR applications and a high nitrogen oxide removal rate in the low-temperature stage. It can be used for denitrification and purification of industrial flue gas in thermal power plants, industrial kilns, cement plants, etc., and is particularly suitable for smoke purification from biomass fuel combustion.
[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: an iron-based loaded low-temperature denitrification catalyst suitable for biomass combustion flue gas, with iron oxide as a carrier, lanthanum manganate as an active ingredient, manganese oxide and lanthanum oxide as active additives, citric acid or oxalic acid as a complexing agent, the molar mass ratio of lanthanum and manganese elements to the complexing agent in the catalyst is 1:1:2 based on metal content, and the loading amount of active substances is 10-40% by mass.
[0007] Preferably, the catalyst is prepared by adding iron oxide to a solution containing a manganese oxide precursor and a lanthanum oxide precursor, and adding a certain amount of a complexing agent, followed by mixing, stirring, drying, igniting, calcining, grinding and screening.
[0008] Preferably, the precursor of manganese oxide is manganese nitrate, and the precursor of lanthanum oxide is lanthanum nitrate.
[0009] Preferably, the iron oxide is γ-type or α-type powder with a particle size of 35 to 65 meshes.
[0010] The method for preparing the iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention comprises the following steps:
[0011] S1, dissolving a precursor of manganese oxide, a precursor of lanthanum oxide, and a complexing agent in deionized water, and placing the mixture in a constant temperature magnetic heating stirrer for water bath heating;
[0012] S2, adding iron oxide powder into the mixed solution of S1, raising the water bath temperature and turning on the rotor, heating and stirring until all the solvent evaporates;
[0013] S3, dripping a small amount of anhydrous ethanol into the gel obtained after evaporation and igniting it until the ethanol is burned out, and then placing it in a drying oven to dry;
[0014] S4, crushing the dried lumps and screening out catalyst particles of a certain mesh size, and calcining them;
[0015] S5. The calcined catalyst is crushed and screened to obtain iron-based supported low-temperature denitration catalyst particles suitable for biomass combustion flue gas.
[0016] Preferably, in step S1, the water bath temperature is 20-50° C., and the water bath time is 10-30 min.
[0017] Preferably, the water bath temperature after the increase in step S2 is 80° C., and the rotor speed is 400-900 r / min.
[0018] Preferably, in step S3, the drying temperature of the drying oven is 100-110° C., and the drying time is 12-15 hours.
[0019] Preferably, in step S4, the calcination temperature is increased from room temperature, the heating rate is 10°C / min, the maximum calcination temperature is 400-550°C, the maximum calcination time is maintained for 3-4 hours, and the total calcination time is 5-6 hours.
[0020] The iron-based supported low-temperature denitration catalyst for biomass combustion flue gas is applied to the purification of biomass fuel combustion smoke, and is particularly applicable to the purification of smoke from thermal power plants, industrial kilns, cement plants and the like.
[0021] Compared with the prior art, the advantages and positive effects of the present invention are: the present invention adopts iron oxide as a carrier, lanthanum manganate as an active component, citric acid as a complexing agent, and does not add toxic and harmful substances. An iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas is prepared by impregnation. The catalyst of the present invention has outstanding effects in SCR applications, a high nitrogen oxide removal rate in the low-temperature stage, and is an environmentally friendly catalyst with simple manufacturing process, low cost, and no secondary pollution when the waste catalyst is recycled. It can be used for smoke purification in thermal power plants, industrial kilns, cement plants and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic structural diagram of a catalyst activity testing device according to an embodiment of the present invention;
[0023] Figure 2 It is a line graph of NOx conversion rate of the catalysts prepared in the examples and comparative examples at different temperatures when testing catalytic activity;
[0024] In the attached figure: 11, NO / N2 mixed gas, 12, O2 / N2 mixed gas, 13, high-purity nitrogen, 14, NH3 / N2 mixed gas, 2, pressure gauge, 3, pressure reducing valve, 4, gas flow meter, 5, mixer, 6, tubular furnace, 7, insulation layer, 8, catalyst layer, 9, filter, 10, flue gas analyzer. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The embodiment of the present invention provides an iron-based loaded low-temperature denitration catalyst suitable for biomass combustion flue gas, with iron oxide as a carrier, lanthanum manganate as an active ingredient, manganese oxide and lanthanum oxide as active aids, citric acid or oxalic acid as a complexing agent, and the molar mass ratio of lanthanum, manganese elements and complexing agents in the catalyst is 1:1:2 in terms of metal content, and the loading amount of active substances is 10-40wt%. The iron-based loaded low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention is prepared by adding iron oxide to a solution containing a precursor of manganese oxide and a precursor of lanthanum oxide, and adding a certain amount of complexing agent, and mixing, stirring, drying, igniting, calcining, grinding, and screening. Among them, the precursor of manganese oxide is manganese nitrate, and the precursor of lanthanum oxide is lanthanum nitrate; iron oxide is γ-type or α-type powder, and the particle size is 35-65 mesh.
[0027] The iron oxide used as a carrier of the iron-based supported low-temperature denitration catalyst for biomass combustion flue gas of the present invention has high specific surface area and chemical stability. Lanthanum manganate used as an active ingredient has a perovskite structure, and perovskite has high specific surface area, stable crystal structure and surface characteristics. Both iron oxide and lanthanum manganate are excellent adsorbents and catalyst carriers. Lanthanum manganate is added to iron oxide powder to form a composite, thereby improving the adsorption capacity and specific surface area of the catalyst and effectively improving the conversion rate of the denitration catalyst.
[0028] The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention comprises the following steps:
[0029] S1. Dissolve the precursor of manganese oxide, the precursor of lanthanum oxide and the complexing agent in a beaker filled with deionized water, and place the beaker in a constant temperature magnetic heating stirrer for water bath, and heat and stir in a constant temperature environment, wherein the water bath temperature is 20-50° C. and the water bath time is 10-30 min;
[0030] S2. According to the calculated loading amount, weigh the required iron oxide powder and put it into the mixed solution of S1. Increase the water bath temperature and turn on the rotor at the same time. Heat and stir until all the solvent is evaporated. The water bath temperature is 80° C. and the rotor speed is 400-900 r / min.
[0031] S3, dripping a small amount of anhydrous ethanol into the gel obtained after evaporation and igniting it, and then placing the dry gel in a drying oven to dry, wherein the drying temperature is 100-110° C. and the drying time is 12-15 hours;
[0032] S4, crushing the lumps obtained after drying and screening out particles with a certain mesh size, and then placing them in a muffle furnace, calcining them in an environment of 400-550° C. for 3-4 hours, wherein the calcination temperature is increased from room temperature, the heating rate is 10° C. / min, the maximum calcination temperature is 400-550° C., the maximum calcination time is maintained for 3-4 hours, and the total calcination time is 5-6 hours;
[0033] S5. Crush and grind the calcined catalyst to select catalyst particles of 35 to 65 mesh.
[0034] The iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas is applied to the purification of biomass fuel combustion smoke, and can be used for smoke purification in thermal power plants, industrial kilns, and cement plants.
[0035] In order to more clearly and in detail introduce the iron-based supported low-temperature denitrification catalyst suitable for biomass combustion flue gas, preparation method and application provided by the embodiments of the present invention, the following description will be combined with specific examples, wherein % in the following embodiments are all mass percentage symbols unless otherwise specified.
[0036] Example 1
[0037] The present embodiment is applicable to the preparation method of the iron-based supported low-temperature denitration catalyst for biomass combustion flue gas, which specifically comprises the following steps:
[0038] Dissolve 2.9g manganese oxide, 5.3g La(NO3)3, and 5.2g citric acid in a beaker filled with 50ml deionized water, and place the beaker in a constant temperature magnetic heating stirrer, adjust the water bath temperature to 30℃, and keep it for 30min to fully dissolve the solute;
[0039] 30 g of γ-type Fe2O3 was added to the above mixed solution, the water bath temperature was raised to 80°C, the rotor speed was adjusted to 450 r / min, and the solution was stirred until the solvent was completely evaporated to obtain a dry gel;
[0040] The dry gel was placed in a crucible, 5 ml of 75% alcohol was added and ignited until the alcohol was burned out, and then placed in a drying oven for drying at a temperature of 105°C for 14 hours;
[0041] The solid catalyst obtained after drying was crushed, ground and screened to obtain particles of 35-65 mesh, and then placed in a muffle furnace for calcination. The temperature was programmed to rise from room temperature (25°C) at a rate of 10°C / min, and after reaching 400°C, the temperature was kept constant for calcination for 3 hours.
[0042] The calcined catalyst is crushed and screened to obtain iron-based supported low-temperature denitration catalyst particles suitable for biomass combustion flue gas.
[0043] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active ingredient LaMnO3 to the carrier iron oxide is 1:10.
[0044] Example 2
[0045] The present embodiment is applicable to the preparation method of the iron-based supported low-temperature denitration catalyst for biomass combustion flue gas, which specifically comprises the following steps:
[0046] Dissolve 9.5g manganese oxide, 17.3g La(NO3)3, and 16.8g citric acid in a beaker filled with 50ml deionized water, and place the beaker in a constant temperature magnetic heating stirrer, adjust the water bath temperature to 30℃, and keep it for 30min to fully dissolve the solute;
[0047] 32.2 g of γ-type Fe2O3 was added to the above mixed solution, the water bath temperature was raised to 80°C, the rotor speed was adjusted to 500 r / min, and the solution was stirred until the solvent was completely evaporated to obtain a dry gel;
[0048] The dry gel was placed in a crucible, 5 ml of 75% alcohol was added and ignited until the alcohol was burned out, and then placed in a drying oven for drying at a temperature of 105°C for 14 hours;
[0049] The solid catalyst obtained after drying was crushed, ground and screened to obtain particles of 35 to 65 mesh, and then placed in a muffle furnace for calcination. The temperature was programmed to rise from room temperature (25°C) at a rate of 10°C / min, and after reaching 500°C, the catalyst was calcined at a constant temperature for 3 hours.
[0050] The calcined catalyst is crushed and screened to obtain iron-based supported low-temperature denitration catalyst particles suitable for biomass combustion flue gas.
[0051] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active ingredient LaMnO3 to the carrier iron oxide is 3:10.
[0052] Example 3
[0053] The present embodiment is applicable to the preparation method of the iron-based supported low-temperature denitration catalyst for biomass combustion flue gas, which specifically comprises the following steps:
[0054] Dissolve 9.5g manganese oxide, 17.3g La(NO3)3, and 16.8g citric acid in a beaker filled with 50ml deionized water, and place the beaker in a constant temperature magnetic heating stirrer, adjust the water bath temperature to 30℃, and keep it for 30min to fully dissolve the solute;
[0055] 24.2 g of γ-type Fe2O3 was added to the above mixed solution, the water bath temperature was raised to 80°C, the rotor speed was adjusted to 500 r / min, and the solution was stirred until the solvent was completely evaporated to obtain a dry gel;
[0056] The dry gel was placed in a crucible, 5 ml of 75% alcohol was added and ignited until the alcohol was burned out, and then placed in a drying oven for drying at a temperature of 105°C for 14 hours;
[0057] The solid catalyst obtained after drying was crushed, ground and screened to obtain particles of 35-65 mesh, and then placed in a muffle furnace for calcination. The temperature was programmed to rise from room temperature (25°C) at a rate of 10°C / min, and after reaching 400°C, the temperature was kept constant for calcination for 3 hours.
[0058] The calcined catalyst is crushed and screened to obtain iron-based supported low-temperature denitration catalyst particles suitable for biomass combustion flue gas.
[0059] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active material LaMnO3 to the carrier iron oxide is 2:5.
[0060] Comparative Example 1
[0061] This comparative example is a LaMnO3 catalyst, and the preparation method specifically includes the following steps:
[0062] Dissolve 9.5g of manganese oxide, 17.3g of La(NO3)3, and 16.8g of citric acid in a beaker filled with 50ml of deionized water, and place the beaker in a constant temperature magnetic heating stirrer, adjust the water bath temperature to 30°C, and stir for 30min to fully dissolve the solute, then increase the water bath temperature to 80°C, adjust the rotor speed to 500r / min, and stir the solution until the solvent is completely evaporated to obtain a catalyst;
[0063] The catalyst was placed in a drying oven and dried at a temperature of 105°C for 14 hours.
[0064] The solid catalyst obtained after drying was crushed, ground and screened to obtain particles of 35 to 65 mesh, and placed in a muffle furnace for calcination. The temperature was programmed to rise from room temperature of 25°C at a rate of 10°C / min. After reaching 400°C, the catalyst was calcined at a constant temperature for 3 hours. The calcined catalyst was crushed and screened to obtain a LaMnO3 catalyst.
[0065] Comparative Example 2
[0066] This comparative example is iron oxide particles with a particle size of 35 to 65 meshes.
[0067] Comparative Example 3
[0068] This comparative example is a V2O5 / Fe2O3 particle with a particle size of 35 to 65 meshes, and the preparation method specifically includes the following steps:
[0069] Dissolve 4.84 g of ammonium metavanadate in a beaker filled with 50 ml of deionized water, and place the beaker in a constant temperature magnetic heating stirrer. Adjust the water bath temperature to 30°C for 30 minutes to allow the solute to fully dissolve.
[0070] 24.2 g of γ-type Fe2O3 was added to the above mixed solution, the water bath temperature was raised to 80°C, the rotor speed was adjusted to 500 r / min, and the solution was stirred until the solvent was completely evaporated to obtain a dry gel;
[0071] The dry gel was placed in a crucible, 5 ml of 75% alcohol was added and ignited until the alcohol was burned out, and then placed in a drying oven for drying at a temperature of 105°C for 14 hours;
[0072] The solid catalyst obtained after drying was crushed, ground and screened to obtain particles of 35-65 mesh, and then placed in a muffle furnace for calcination. The temperature was programmed to rise from room temperature (25°C) at a rate of 10°C / min, and after reaching 400°C, the temperature was kept constant for calcination for 3 hours.
[0073] The calcined catalyst is crushed and screened to obtain supported vanadium-based low-temperature denitration catalyst particles.
[0074] In terms of metal content, in the catalyst prepared in this comparative example, the mass ratio of the active substance V2O3 to the carrier iron oxide is 2:5.
[0075] Performance Testing
[0076] use Figure 1 The catalyst activity test device shown in the figure measures the activity of the catalysts prepared in Examples 1-3 and Comparative Examples 1-3, and the test conditions are:
[0077] Airspeed: 7500h -1 ; O2 intake content: 3%; NO intake content: 500ppm; SO2 intake content: 100ppm; H2O intake content: 1%; NH3 / NO=1:1; Temperature: 90℃, 120℃, 150℃, 180℃, 210℃, 240℃, 270℃, 300℃, 330℃;
[0078] The specific test method includes the following steps:
[0079] (1) Loading the catalyst: Weigh the catalyst with a measuring cylinder and load it into a quartz tube;
[0080] (2) Preheating of flue gas analyzer: After the experimental device is powered on, turn on the flue gas analyzer and preheat it for 20 minutes to allow it to reach a stable working state;
[0081] (3) Tube furnace temperature program setting: Turn on the power of the experimental bench thermostat, set the tube furnace temperature rise rate, reaction temperature and dwell time of each reaction temperature, open the N2 gas valve, and when the temperature rises to the set reaction temperature, the thermostat will perform the insulation-heating-insulation stage according to the preset program;
[0082] (4) Reaction gas introduction: Open the NOx valve and introduce gas. The gas flow is controlled and adjusted by the gas distribution system. When the NOx concentration at the reactor outlet is stable, record the NOx inlet concentration c at this time. NO进口 ;
[0083] (5) NOx outlet concentration detection: When reaching each temperature measurement point, the heating program will enter a constant temperature state. When the NOx reading in the flue gas analyzer is stable, the NOx outlet concentration c at this time is recorded. NO出口 ;
[0084] (6) Program heating: follow the preset heating program to the next temperature range and repeat steps (4) and (5);
[0085] (7) When the temperature is adjusted to the test temperature and the catalytic denitrification efficiency is stable for 100 minutes, open the SO2 valve and introduce H2O, and record the NOx outlet concentration c every 10 minutes. NO出口 , continue to flow for 400 minutes to cut off SO2 and H2O, then record the NOx outlet concentration, and continue the test for 100 minutes;
[0086] (8) Calculate the NOx conversion rate.
[0087] Component analysis: The denitrification performance of the catalyst and its alkaline resistance were studied based on a 0.5% K2O loading.
[0088] The NO concentration in the sample was measured using a flue gas analyzer, and the NO conversion rate was calculated as follows:
[0089]
[0090] Where η NO is NO conversion rate; c NO进口 is the inlet concentration of NO; c NO出口 is the NO outlet concentration; for trace reaction, the volume change is negligible. The measurement results are shown in Table 1 below. The line graph obtained by drawing Table 1 is shown in Figure 2 shown.
[0091] Table 1 Denitrification efficiency of supported iron-based low-temperature denitrification catalyst at different temperatures in the examples and comparative examples
[0092]
[0093] As can be seen from Table 1, Comparative Example 1 is a catalyst without iron oxide loading, and its denitration efficiency is very high in the low temperature section of 150-210°C, but its temperature window is narrow; Comparative Example 2 is an iron oxide catalyst, and its denitration performance is poor at less than 240°C (low temperature section); Comparative Example 3 is a V2O5 / Fe2O3 catalyst, and its denitration efficiency in the temperature range of 90°C to 330°C is lower than that of Examples 1-3 of the present invention. Examples 1-3 have higher denitration efficiency than Comparative Examples 2 and Comparative Examples 3 in the low temperature section of 90-210°C, indicating that in the low temperature section, the denitration performance of the catalyst of the present invention is better than that of the iron oxide catalyst (Comparative Example 2) and the vanadium-based catalyst (Comparative Example 3).
[0094] The supported iron-based low-temperature denitration catalyst prepared in Example 1 of the present invention has a denitration efficiency of more than 80% at 210°C to 330°C; the supported iron-based low-temperature denitration catalysts prepared in Examples 2 and 3 have a denitration efficiency of more than 80% at 180 to 330°C; however, the temperature range for maintaining a denitration efficiency of 80% in Comparative Example 1 is 150 to 210°C, and the temperature range for maintaining a denitration efficiency of 80% in Comparative Example 2 is 210°C to 330°C. It can be seen that the iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention has a better low-temperature catalytic effect, and the high-activity temperature window of the iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention is relatively wide.
[0095] The above-described embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions, and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the scope of protection determined by the claims of the present invention.
Claims
1. An iron-based supported low-temperature denitrification catalyst suitable for biomass combustion flue gas, It is characterized in that The catalyst uses iron oxide as a carrier, lanthanum manganate as an active ingredient, manganese oxide and lanthanum oxide as active aids, citric acid or oxalic acid as a complexing agent, and based on metal content, the molar mass ratio of lanthanum, manganese elements and complexing agent in the catalyst is 1:1:2, and the loading amount of active substances is 10-40%.
2. The iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 1, It is characterized in that The catalyst is prepared by adding iron oxide to a solution containing a manganese oxide precursor and a lanthanum oxide precursor, and adding a certain amount of a complexing agent, and then mixing, stirring, drying, igniting, calcining, grinding and screening.
3. The iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 2, It is characterized in that The precursor of manganese oxide is manganese nitrate, and the precursor of lanthanum oxide is lanthanum nitrate.
4. The iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 1, It is characterized in that The iron oxide is γ-type or α-type powder with a particle size of 35 to 65 meshes.
5. The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1, dissolving a precursor of manganese oxide, a precursor of lanthanum oxide, and a complexing agent in deionized water, and placing the mixture in a constant temperature magnetic heating stirrer for water bath heating; S2, adding iron oxide powder into the mixed solution of S1, raising the water bath temperature and turning on the rotor, heating and stirring until all the solvent evaporates; S3, dripping a small amount of anhydrous ethanol into the gel obtained after evaporation and igniting it until the ethanol is burned out, and then placing it in a drying oven to dry; S4, crushing the dried block and screening out catalyst particles of a certain mesh size, and calcining; S5. The calcined catalyst is crushed and screened to obtain iron-based supported low-temperature denitration catalyst particles suitable for biomass combustion flue gas.
6. The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 5, It is characterized in that In step S1, the water bath temperature is 20-50° C., and the water bath time is 10-30 min.
7. The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 5, It is characterized in that After the water bath temperature is increased in step S2, it is 80°C and the rotor speed is 400-900 r / min.
8. The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 5, It is characterized in that In step S3, the drying temperature of the drying oven is 100-110° C., and the drying time is 12-15 hours.
9. The method for preparing an iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 5, It is characterized in that In step S4, the calcination temperature is increased from room temperature, the heating rate is 10°C / min, the maximum calcination temperature is 400-550°C, the maximum calcination time is maintained for 3-4 hours, and the total calcination time is 5-6 hours.
10. Use of the iron-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to any one of claims 1 to 4 in denitration during the purification of biomass fuel combustion smoke.
Citation Information
Patent Citations
Application of natural spathic iron in preparation of SCR denitration catalyst
CN104307533A
Preparing and testing method of medium-low-temperature loaded denitration catalyst taking raw iron ore as carrier
CN105214670A