Supported high-entropy catalyst as well as preparation method and application thereof

Through the immersion method and reduction treatment of the supported high-entropy catalyst, combined with the high-entropy active component and the titanium dioxide support, the problems of low efficiency and high energy consumption of the existing catalysts under low temperature and low pressure conditions are solved, and efficient and stable CO2 addition is achieved The hydrogen and CO oxidation reaction meets the 'dual carbon' target of energy consumption reduction and catalytic efficiency improvement.

CN118892846AActive Publication Date: 2024-11-05TSINGHUA UNIVERSITY

Patent Information

Application Number
CN202410777793.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-05
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

The existing CO2 catalysts are low in catalytic efficiency under low temperature and low pressure conditions, and the high-temperature active sites are easy to sinter, which limits their industrial applications. The precious metal catalysts are costly and complex in preparation, making it difficult to meet the energy consumption reduction and catalytic efficiency of the 'dual carbon' target. Increase demand.

Method used

Supported high-entropy catalysts, including high-entropy active components (indium, cobalt, nickel, zinc, ruthenium, etc.) and titanium dioxide support, are prepared by impregnation and reduction treatment to avoid high-temperature calcination and achieve low energy consumption and high-efficiency catalysis.

Benefits of technology

It demonstrates excellent catalytic performance and stability in CO2 hydrogenation and CO oxidation reactions, and the preparation method is simple, with low energy consumption and high yield, meeting the catalytic requirements under low temperature and low pressure conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892846A_ABST
    Figure CN118892846A_ABST
Patent Text Reader

Abstract

The invention discloses a supported high-entropy catalyst and a preparation method and application thereof, the supported high-entropy catalyst comprises a high-entropy active component and a titanium dioxide carrier, the high-entropy active component contains any four of indium, cobalt, nickel, zinc, aluminum and ruthenium and copper, and the average particle size of the titanium dioxide carrier is 100-150 nm. Therefore, the supported high-entropy catalyst has excellent catalytic performance and stability in CO2 hydrogenation and CO oxidation reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and specifically relates to a supported high-entropy catalyst and a preparation method and application thereof. Background Art

[0002] Currently, CO is widely used 2 Catalytic conversion technology is a process of converting CO into 2 Converted into high value-added chemicals, such as methane, methanol, ethylene, etc. The CuO-ZnO-Al 2 O 3 (CuZnAl) catalyst has excellent catalytic performance under the conditions of 220℃-240℃ and 5MPa-10MPa. Based on the excellent catalytic performance and low cost of CuZnAl catalyst, CO 2 The development and modification of hydrogenation catalysts are still centered around CuZnAl catalysts, especially by optimizing the physical and chemical properties of the Cu base to improve its low-temperature performance and stability. 2 Research reports on hydrogenation catalysts have been published, but their high cost, complex preparation process and the easy sintering of active sites at high temperatures also limit their application in the industrial field. In addition, with the proposal and implementation of the "dual carbon" goal, in addition to converting CO 2 In addition to converting into high-value-added chemicals, optimizing reaction conditions (such as low temperature and low pressure) at the user end to reduce energy consumption while ensuring catalytic efficiency is also an important development direction.

[0003] High-entropy materials (high-entropy oxides and high-entropy alloys) have abundant active sites, stable crystal structures, unique geometric compatibility and electronic structures, and can catalyze CO 2 The hydrogenation reaction can also catalyze the CO oxidation reaction. Therefore, it is urgent to develop a catalyst based on high entropy materials. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one object of the present invention is to provide a supported high entropy catalyst and a preparation method and application thereof, wherein the supported high entropy catalyst can adjust the spatial position of the high entropy active component and the titanium dioxide carrier to optimize the physicochemical properties of the high entropy component, 2 It has excellent catalytic performance and stability in hydrogenation and CO oxidation reactions, and its preparation method is simple, does not require high-temperature calcination, has low energy consumption and high yield.

[0005] In the first aspect of the present invention, the present invention proposes a supported high entropy catalyst, comprising a high entropy active component and a titanium dioxide carrier; the high entropy active component contains any four of indium, cobalt, nickel, zinc, aluminum, ruthenium and copper; the average particle size of the titanium dioxide carrier is 100nm-150nm. 2 It has excellent catalytic performance and stability in hydrogenation and CO oxidation reactions.

[0006] According to one embodiment of the present invention, based on the total amount of the high entropy active component, the copper accounts for 17.2%-23.8%; and / or, the indium accounts for 19.1%-20.7%; and / or, the cobalt accounts for 19.1%-20.7%; and / or, the nickel accounts for 19.1%-20.7%; and / or, the zinc accounts for 19.1%-20.7%; and / or, the ruthenium accounts for 19.1%-20.7%. Thus, the supported high entropy catalyst is in CO 2 It has excellent catalytic performance and stability in hydrogenation and CO oxidation reactions.

[0007] According to one embodiment of the present invention, the high entropy active component contains copper, cobalt, nickel, zinc and ruthenium. Thus, the catalyst can further react with CO 2 Adsorption and activation are carried out, which is beneficial to CO 2 Hydrogenation catalytic reaction.

[0008] According to one embodiment of the present invention, the molar ratio of copper, cobalt, nickel, zinc and ruthenium in the high entropy active component is 1:(0.8-1.2):(0.8-1.2):(0.8-1.2):(0.8-1.2). Thus, the catalyst can further react with CO 2 Adsorption and activation are carried out, which is more conducive to CO 2 Hydrogenation catalytic reaction.

[0009] According to one embodiment of the present invention, the crystalline phase of the titanium dioxide carrier is anatase, and the anatase phase titanium dioxide has a large surface area and a stable structure. Thus, the supported high entropy catalyst can be evenly dispersed on the surface of the carrier.

[0010] According to one embodiment of the present invention, based on the mass of the titanium dioxide carrier, the mass fraction of the high entropy active component in the titanium dioxide carrier is 10%-18%. Thus, the supported high entropy catalyst can be dispersed in a single layer or a few layers on the carrier surface.

[0011] In a second aspect of the present invention, the present invention provides a method for preparing the supported high entropy catalyst described in the first aspect, comprising:

[0012] (1) preparing an inorganic salt precursor of a high entropy active component into a solution;

[0013] (2) impregnating the solution into a titanium dioxide support and drying the support to obtain a supported high entropy catalyst precursor;

[0014] (3) Reducing the supported high entropy catalyst precursor to obtain a supported high entropy catalyst.

[0015] Therefore, the method for preparing a supported high-entropy catalyst according to the present invention adopts an impregnation method and a reduction treatment, and the method is simple, does not require high-temperature calcination, has low energy consumption, and has a high yield.

[0016] According to one embodiment of the present invention, in step (1), the inorganic salt precursor of the active component includes at least one of nitrate, sulfate or chloride, thereby promoting the rapid decomposition of anionic species in the subsequent reduction process and achieving low-temperature generation of high-entropy components.

[0017] According to one embodiment of the present invention, in step (2), the temperature of the drying treatment is 90° C.-120° C. Thus, it is possible to generate high entropy components at a relatively low temperature.

[0018] According to one embodiment of the present invention, in step (2), the drying time is 6 hours to 12 hours, thereby enabling the generation of high entropy components in a relatively short time.

[0019] According to one embodiment of the present invention, in step (3), the temperature of the reduction treatment is 200° C.-500° C. Thus, the reduction preparation of the supported high entropy catalyst at a relatively low temperature can be achieved.

[0020] According to one embodiment of the present invention, in step (3), the heating rate of the reduction treatment is 3°C / min-5°C / min. Thus, rapid thermal bonding between different metals can be avoided, thereby achieving the formation of high entropy components.

[0021] According to one embodiment of the present invention, in step (3), the reduction treatment time is 2h-4h. Thus, the formation of high entropy components can be achieved in a short time, and the sintering and agglomeration of high entropy components can be avoided.

[0022] In the third aspect of the present invention, the present invention provides a method for treating a mixed gas containing carbon monoxide and oxygen, wherein the mixed gas containing carbon monoxide and oxygen is mixed with the catalyst described in the first aspect or the catalyst prepared by the method described in the second aspect. Thus, the catalyst described in the present invention has excellent catalytic performance and stability in the CO oxidation reaction.

[0023] In a fourth aspect of the present invention, a method for treating a mixed gas containing carbon dioxide and hydrogen is provided, wherein the mixed gas containing carbon dioxide and hydrogen is mixed with the catalyst described in the first aspect or the catalyst prepared by the method described in the second aspect. 2 It has excellent catalytic performance and stability in hydrogenation reactions.

[0024] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0026] Figure 1 The present invention is a flow chart of a method for preparing a supported high entropy catalyst according to an embodiment of the present invention.

[0027] Figure 2 is the H of the supported high entropy catalyst of Example 1 of the present invention 2 -TPR spectrum.

[0028] Figure 3 3 is a scanning electron microscope image of the supported high entropy catalyst of Example 1 of the present invention, wherein the portion marked with a red circle is the formed high entropy active component.

[0029] Figure 4 is the CO of the supported high entropy catalyst of Example 1 of the present invention 2 -TPD curve graph. DETAILED DESCRIPTION

[0030] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.

[0031] In the first aspect of the present invention, the present invention proposes a supported high entropy catalyst, comprising a high entropy active component and a titanium dioxide carrier; the high entropy active component contains any four of indium, cobalt, nickel, zinc, aluminum, ruthenium and copper; the average particle size of the titanium dioxide carrier is 100nm-150nm.

[0032] The inventors found that when the carrier particle size is small (<100nm), the high entropy component formed during the reduction process is small due to the small support surface of the carrier, so that the high entropy component agglomerates between the carrier pores, resulting in poor catalytic performance. In the case of a larger carrier particle size (100nm-150nm), the high entropy component formed is relatively evenly dispersed on the carrier surface. By adjusting the titanium dioxide carrier particle size (100nm-150nm), the spatial configuration of the high entropy component and titanium dioxide can be optimized. At the same time, a small-sized high entropy component can be obtained, and the interaction between the high entropy component and the titanium dioxide carrier can be improved. When the carrier particle size is further increased (>150nm), the high entropy components formed on the carrier surface are far apart and have weak interactions, and their catalytic performance will also decrease. In addition, the titanium dioxide carrier easily induces the occurrence of the hydrogen overflow effect, thereby promoting the reduction and generation of high entropy components and CO 2 Therefore, based on the improvement of the spatial configuration of the high entropy component and the titanium dioxide carrier, the physicochemical properties of the high entropy component can be optimized, so that the supported high entropy catalyst can be used in CO 2 It exhibits excellent catalytic performance and stability in both hydrogenation and CO oxidation reactions.

[0033] According to one embodiment of the present invention, based on the total amount of the high entropy active component, the copper accounts for 17.2%-23.8%, for example, it can be 17.2%, 18.7%, 19.5%, 20.2%, 21.7%, 22.5%, 23.8%, etc.; and / or, the indium accounts for 19.1%-20.7%, for example, it can be 19.1%, 19.7%, 20.2%, 20.7%, etc.; and / or, the cobalt accounts for 19.1%-20.7%, for example, it can be 19.1 %, 19.7%, 20.2%, 20.7%, etc.; and / or, the nickel accounts for 19.1%-20.7%, for example, 19.1%, 19.7%, 20.2%, 20.7%, etc.; and / or, the zinc accounts for 19.1%-20.7%, for example, 19.1%, 19.7%, 20.2%, 20.7%, etc.; and / or, the ruthenium accounts for 19.1%-20.7%, for example, 19.1%, 19.7%, 20.2%, 20.7%, etc. Thus, the supported high entropy catalyst is 2 It has excellent catalytic performance and stability in hydrogenation and CO oxidation reactions.

[0034] According to one embodiment of the present invention, the high entropy active component contains copper, cobalt, nickel, zinc and ruthenium, wherein the copper and zinc components are conducive to CO 2 During the adsorption process, the cobalt and nickel components are beneficial to the hydrogenation process, and the ruthenium component can increase the hydrogen overflow effect. Thus, the supported high entropy catalyst contains copper, cobalt, nickel, zinc and ruthenium, which can further react with CO2 Adsorption and activation are carried out, which is beneficial to CO 2 Hydrogenation catalytic reaction.

[0035] According to one embodiment of the present invention, the molar ratio of copper, cobalt, nickel, zinc and ruthenium in the high entropy active component is 1:(0.8-1.2):(0.8-1.2):(0.8-1.2):(0.8-1.2), for example, it can be 1:0.9:0.9:0.9:0.9, 1:1:1:1:1, 1:1.1:1.1:1.1:1.1, etc. Thus, by controlling the molar ratio of copper, cobalt, nickel, zinc and ruthenium in the high entropy active component within the above range, it can be further combined with CO 2 Adsorption and activation are carried out, which is more conducive to CO 2 Hydrogenation catalytic reaction.

[0036] According to one embodiment of the present invention, the titanium dioxide carrier crystal phase is anatase. Thus, the supported high entropy catalyst can promote the dispersion of high entropy components and the catalytic stability.

[0037] According to one embodiment of the present invention, based on the mass of the titanium dioxide carrier, the mass fraction of the high entropy active component in the titanium dioxide carrier is 10%-18%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, etc. Thus, by adjusting the mass fraction of the high entropy active component in the titanium dioxide carrier within the above range, it is possible to avoid aggregation caused by the high entropy component, ensure higher catalytic sites, ensure a suitable spatial distance between high entropy components, facilitate the migration and conversion of adsorbed active species, and thus improve the catalytic performance. Therefore, the mass fraction of the high entropy active component in the titanium dioxide carrier of the present invention is 10%-18%, which can achieve the maximum improvement of catalytic performance.

[0038] In a second aspect of the present invention, the present invention provides a method for preparing the supported high entropy catalyst described in the first aspect, referring to Figure 1 ,include:

[0039] S100: Preparing the inorganic salt precursor of the high entropy active component into a solution

[0040] In this step, an inorganic salt precursor of a high entropy active component is prepared into a solution.

[0041] According to one embodiment of the present invention, in S100, the inorganic salt precursor of the active component includes at least one of nitrate, sulfate or chloride, for example, copper nitrate, cobalt chloride, nickel nitrate, zinc nitrate, indium nitrate, ruthenium trichloride, etc., thereby enabling the decomposition of anionic species during the reduction and heating process.

[0042] According to one embodiment of the present invention, in S100, the inorganic salt precursor of the high entropy active component is prepared as an aqueous solution.

[0043] According to one embodiment of the present invention, in S100, the molar concentration of the inorganic salt precursor solution is 60mmol / L-140mmol / L, for example, it can be 60mmol / L, 70mmol / L, 80mmol / L, 90mmol / L, 100mmol / L, 110mmol / L, 120mmol / L, 130mmol / L, 140mmol / L, etc.

[0044] S200: impregnating the solution into a titanium dioxide carrier and drying to obtain a supported high entropy catalyst precursor

[0045] In this step, the solution is impregnated into a titanium dioxide support, and then dried to obtain a supported high entropy catalyst precursor. Thus, the method for preparing a supported high entropy catalyst of the present invention adopts an impregnation method, which is simple, does not require high-temperature calcination, has low energy consumption, and has a high yield.

[0046] According to one embodiment of the present invention, in S200, the drying temperature is 90°C-120°C, for example, 90°C, 100°C, 110°C, 120°C, etc. Thus, it is possible to generate high entropy components at a relatively low temperature.

[0047] According to one embodiment of the present invention, in S200, the drying process lasts for 6 hours to 12 hours, for example, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, etc. Thus, the volatilization of water can be achieved in a shorter time.

[0048] According to one embodiment of the present invention, in S200, the impregnation method can be a step-by-step equal volume impregnation method, specifically, an equal volume of high entropy component solution is impregnated into a titanium dioxide carrier and then allowed to stand and dry, and then the equal volume impregnation and drying is cyclically performed until all the solution is impregnated. After the impregnation is completed, each standing treatment time is 60 minutes, and each infrared lamp heat treatment time is 30 minutes.

[0049] According to one embodiment of the present invention, in S200, the drying may be vacuum drying, the vacuum drying treatment temperature is 90° C.-120° C., and the vacuum drying treatment time is 6 h-12 h.

[0050] S300: reducing the supported high entropy catalyst precursor to obtain a supported high entropy catalyst

[0051] In this step, the supported high entropy catalyst precursor is reduced to obtain a supported high entropy catalyst. Therefore, the method for preparing a supported high entropy catalyst of the present invention adopts an impregnation method and a reduction treatment, and realizes the low-temperature formation of a high entropy component by means of a hydrogen overflow effect during the reduction process. The method is simple, does not require high-temperature calcination, has low energy consumption, and has a high yield.

[0052] According to one embodiment of the present invention, in S300, the temperature of the reduction treatment is 200°C-500°C, for example, 200°C, 300°C, 400°C, 500°C, etc. Thus, the reduction preparation of the supported high entropy catalyst at a lower temperature is achieved by introducing the precious metal components (any four of indium, cobalt, nickel, zinc, aluminum, ruthenium and copper).

[0053] According to one embodiment of the present invention, in S300, the heating rate of the reduction treatment is 3°C / min-5°C / min, for example, 3°C / min, 4°C / min, 5°C / min, etc. Thus, rapid thermal bonding between different metals can be avoided, thereby achieving the formation of high entropy components.

[0054] According to one embodiment of the present invention, in S300, the reduction treatment time is 2h-4h, for example, 2h, 3h, 4h, etc. Thus, the formation of high entropy components can be achieved in a short time, and the sintering and agglomeration of high entropy components can be avoided.

[0055] According to one embodiment of the present invention, in S300, the reduction method can be directly reducing with hydrogen to obtain a supported high-entropy catalyst, or it can be directly used for catalytic reaction after reduction treatment on an active device (such as a fixed bed reactor, a tubular furnace, etc.).

[0056] According to a specific embodiment of the present invention, the method for preparing the supported high entropy catalyst is: adding an inorganic salt precursor of a high entropy component to water in equal moles to prepare a mixed metal solution, then adding the mixed metal solution to a titanium dioxide carrier by a step-by-step equal volume impregnation method, and combining the method of standing, infrared lamp irradiation and vacuum drying to obtain a catalyst precursor. Finally, the supported high entropy catalyst is obtained by hydrogen reduction treatment.

[0057] Therefore, the method for preparing a supported high-entropy catalyst according to the present invention adopts an impregnation method and a reduction treatment, and the method is simple, does not require high-temperature calcination, has low energy consumption, and has a high yield.

[0058] In the third aspect of the present invention, the present invention provides a method for treating a mixed gas containing carbon monoxide and oxygen, wherein the mixed gas containing carbon monoxide and oxygen is mixed with the catalyst described in the first aspect or the catalyst prepared by the method described in the second aspect. Thus, the catalyst described in the present invention has excellent catalytic performance and stability in the CO oxidation reaction.

[0059] According to one embodiment of the present invention, in the mixed gas of carbon monoxide and oxygen, the volume ratio of carbon monoxide to oxygen is 1:10; the flow rate of the mixed gas is 100mL / min-300mL / min; the mass of the catalyst is 0.1g-0.2g; and the temperature of the mixed reaction of the mixed gas of carbon monoxide and oxygen and the catalyst is 50℃-300℃.

[0060] In a fourth aspect of the present invention, a method for treating a mixed gas containing carbon dioxide and hydrogen is provided, wherein the mixed gas containing carbon dioxide and hydrogen is mixed with the catalyst described in the first aspect or the catalyst prepared by the method described in the second aspect. 2 It has excellent catalytic performance and stability in hydrogenation reactions.

[0061] According to one embodiment of the present invention, in the mixed gas containing carbon dioxide and hydrogen, the volume ratio of carbon dioxide to hydrogen is 4:1; the flow rate of the mixed gas is 50mL / min-100mL / min; the mass of the catalyst is 0.2-0.5g; and the temperature of the mixed reaction of the mixed gas of carbon dioxide and hydrogen and the catalyst is 200℃-550℃.

[0062] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0063] In the following examples, the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased from the market.

[0064] Example 1

[0065] Weigh 0.4832 g of copper nitrate hexahydrate, 0.4758 g of cobalt chloride hexahydrate, 0.5816 g of nickel nitrate hexahydrate, 0.5950 g of zinc nitrate hexahydrate, and 0.7254 g of ruthenium trichloride, respectively, and transfer them to 16.6 mL of deionized water to prepare a 120 mM mixed solution, which is recorded as solution L3. Weigh 4 g of TiO 2 (anatase crystal form) carrier in a polytetrafluoroethylene beaker, TiO 2 The particle size was 100 nm. The L3 solution (12.1 mL) was added to TiO 2In the carrier, after each step of saturation, the solution was allowed to stand for 110 minutes, and then dried with an infrared lamp for 50 minutes. After the solution was used up, it was transferred to a vacuum drying oven and treated at 110°C for 10 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 200°C for 3 hours (heating rate of 2°C / min) was a supported high-entropy catalyst, denoted as catalyst M1, and the mass fraction of the high-entropy component in catalyst M1 was 12% of the carrier.

[0066] refer to Figure 2 , H of the supported high entropy catalyst of Example 1 2 -TPR spectrum shows that the catalyst prepared in Example 1 has a sharp reduction peak at low temperature and a gentle reduction peak at high temperature, indicating that the high entropy catalyst on the carrier surface is formed by reduction.

[0067] refer to Figure 3 , Figure 2 is a scanning electron microscope image of the supported high entropy catalyst of Example 1 of the present invention, wherein the red circled portion is the formed high entropy active component. Figure 2 It can be seen that the high entropy component formed in the catalyst prepared in Example 1 is relatively evenly dispersed on the surface of the carrier.

[0068] refer to Figure 4 , CO of the supported high entropy catalyst of Example 1 2 -TPD curve shows that the catalyst surface prepared in Example 1 has an obvious low-temperature CO 2 The desorption peak (115°C) and an obvious high temperature CO 2 Desorption peak (762℃).

[0069] Example 2

[0070] Weigh 0.4832 g of copper nitrate hexahydrate, 0.5820 g of cobalt nitrate hexahydrate, 0.5816 g of nickel nitrate hexahydrate, 0.6012 g of indium nitrate, and 0.7254 g of ruthenium trichloride, and transfer them to 14.3 mL of deionized water to prepare a 140 mM mixed solution, which is recorded as solution L4. Weigh 4 g of TiO 2 (anatase crystal form) carrier in a polytetrafluoroethylene beaker, TiO 2 The particle size of the TiO 2In the carrier, after each step of saturation, the solution was allowed to stand for 120 minutes, and then dried with an infrared lamp for 60 minutes. After the solution was used up, it was transferred to a vacuum drying oven and treated at 120°C for 12 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 400°C for 3 hours (heating rate of 3°C / min) was a supported high-entropy catalyst, denoted as catalyst M2, and the mass fraction of the high-entropy component in catalyst M2 was 18%.

[0071] Example 3

[0072] Example 3 was carried out in the same manner as Example 1, except that in Example 3, TiO 2 The particle size is 120 nm, and the obtained supported high entropy catalyst is recorded as catalyst M3.

[0073] Comparative Example 1

[0074] The metal precursors in the high entropy component were weighed in equal moles, specifically 0.9664 g of copper nitrate hexahydrate, 1.1640 g of cobalt nitrate hexahydrate, 1.1632 g of nickel nitrate hexahydrate, 1.1900 g of zinc nitrate hexahydrate and 1.4928 g of aluminum nitrate hexahydrate, and then transferred to a mortar for grinding for 30 minutes until uniform and free of particles. The ground mixture was then placed in a crucible and transferred to a muffle furnace and reacted at 900 ° C for 4 hours (heating rate of 3 ° C / min). After the reaction was completed, the black product was cooled to room temperature to obtain a high entropy oxide, which was recorded as catalyst D1.

[0075] Comparative Example 2

[0076] 0.24 g of catalyst D1 was weighed and ground until there was no particle feeling, and then 100 mL of deionized water was added to prepare a solution. Then, the prepared solution was impregnated in equal volumes in 2 g of TiO 2 Support surface, TiO 2 The particle size is 100 nm, and then it is placed in an infrared lamp (50 minutes) and a vacuum drying oven (100°C, 10 hours) for heat treatment. The obtained supported catalyst is recorded as catalyst D2. The mass fraction of the high entropy component in catalyst D2 is 24%.

[0077] Comparative Example 3

[0078] Weigh 0.4832 g of copper nitrate hexahydrate, 0.4758 g of cobalt chloride hexahydrate, 0.5816 g of nickel nitrate hexahydrate, 0.5950 g of zinc nitrate hexahydrate, and 0.7464 g of aluminum nitrate nonahydrate, and transfer them to 25 mL of deionized water to prepare a mixed solution of 80 mM, which is recorded as solution L1. Weigh 4 g of TiO 2 The support (anatase crystal form) was placed in a polytetrafluoroethylene beaker, and the TiO 2The particle size was 30 nm. The L1 solution (11.12 mL) was added to the TiO 2 In the carrier, after each step of saturation, the solution was allowed to stand for 90 minutes, and then dried with an infrared lamp for 30 minutes. After the solution was used up, it was transferred to a vacuum drying oven and treated at 90°C for 6 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 350°C for 2 hours (heating rate of 4°C / min) was a supported high-entropy catalyst, denoted as catalyst D3, in which the high-entropy component in catalyst D3 accounted for 6% of the carrier mass fraction.

[0079] Comparative Example 4

[0080] Weigh 0.4832 g of copper nitrate hexahydrate, 0.5820 g of cobalt nitrate hexahydrate, 0.6012 g of indium nitrate, 0.5391 g of zinc sulfate hexahydrate, and 0.7464 g of aluminum nitrate nonahydrate, and transfer them to 33 mL of deionized water to prepare a 60 mM mixed solution, which is recorded as solution L2. Weigh 4 g of TiO 2 (anatase crystal form) carrier in a polytetrafluoroethylene beaker, TiO 2 The particle size was 60 nm. The L2 solution (16.02 mL) was added to the TiO 2 In the carrier, after each step of saturation, the solution was allowed to stand for 60 minutes, and then dried with an infrared lamp for 40 minutes. After the solution was used up, it was transferred to a vacuum drying oven and treated at 100°C for 8 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 500°C for 2 hours (heating rate of 5°C / min) was a supported high-entropy catalyst, denoted as catalyst D4, in which the high-entropy component in catalyst D4 accounted for 8% of the carrier mass fraction.

[0081] Comparative Example 5

[0082] Weigh 4 g of alumina support into a polytetrafluoroethylene beaker. 2 O 3 The particle size was 100 nm. The L3 solution (12.1 mL) was added to the Al 2 O 3 In the carrier, after each step of saturation, the solution was allowed to stand for 110 minutes, and then dried with an infrared lamp for 50 minutes. After the solution was used up, it was transferred to a vacuum drying oven and treated at 110°C for 10 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 200°C for 3 hours (heating rate of 2°C / min) was a supported high-entropy catalyst, denoted as catalyst D5, in which the high-entropy component in catalyst D5 accounted for 12% of the carrier mass fraction.

[0083] Comparative Example 6

[0084] Weigh 0.4832 g of copper nitrate hexahydrate, 0.4758 g of cobalt chloride hexahydrate, 0.5816 g of nickel nitrate hexahydrate, 0.5950 g of zinc nitrate hexahydrate, 0.6012 g of indium nitrate and 0.7254 g of ruthenium trichloride respectively, and then transfer them into 16.6 mL of deionized water to prepare a 120 mM mixed solution, which is recorded as solution L5. Weigh 4 g of TiO 2 (anatase crystal form) carrier in a polytetrafluoroethylene beaker, TiO 2 The particle size was 100 nm. The L5 solution (12.1 mL) was added to the TiO 2 In the carrier, each step of impregnation was allowed to stand for 110 minutes, followed by drying with an infrared lamp for 50 minutes, and after the solution was used up, it was transferred to a vacuum drying oven and treated at 110°C for 10 hours to obtain a supported high-entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 200°C for 3 hours (heating rate of 2°C / min) was a supported high-entropy catalyst, denoted as catalyst D6, in which the mass fraction of the high-entropy component in the carrier was 14%.

[0085] Comparative Example 7

[0086] Weigh 0.4832 g of copper nitrate hexahydrate, 0.4758 g of cobalt chloride hexahydrate, 0.5816 g of nickel nitrate hexahydrate, 0.5950 g of zinc nitrate hexahydrate, and 0.7254 g of ruthenium trichloride, respectively, and transfer them to 16.6 mL of deionized water to prepare a 120 mM mixed solution, which is recorded as solution L3. Weigh 4 g of TiO 2 (anatase crystal form) carrier in a polytetrafluoroethylene beaker, TiO 2 The particle size was 200 nm. The L3 solution (12.1 mL) was added to TiO 2 In the carrier, each step of impregnation was allowed to stand for 110 minutes, followed by drying with an infrared lamp for 50 minutes, and after the solution was used up, it was transferred to a vacuum drying oven and treated at 110°C for 10 hours to obtain a supported high entropy catalyst precursor. The black product obtained after further reduction treatment with hydrogen at 200°C for 3 hours (heating rate of 2°C / min) was a supported high entropy catalyst, denoted as catalyst D7, in which the high entropy component in catalyst D7 accounted for 12% of the carrier mass fraction.

[0087] Test Case

[0088] 1. CO 2 Hydrogenation activity test

[0089] The catalysts of the above examples and comparative examples were applied to CO 2 Hydrogenation activity test, the activity and stability results of the catalyst are based on CO 2The conversion rate indicates that CO 2 Conversion rate (%) = (CO 2 Inlet-CO 2 Export) / CO 2 Inlet × 100%, CO 2 The concentration was tested using online chromatography, and the results are shown in Table 1 below.

[0090] CO 2 The conditions for the hydrogenation activity test are: the catalyst loading is 0.2 g, the reaction temperature is 200°C-550°C, the CO 2 / H 2 (v / v=1:4) The mixed gas flow rate is 100 mL / min, of which CO 2 The volume fraction is 4%.

[0091] CO 2 The hydrogenation stability test was carried out in the same device, and the test conditions were: catalyst loading was 0.2 g, reaction temperature was 400 °C, feed gas flow rate was 100 mL / min, and long-term stability test time was 50 h.

[0092] Table 1 CO of supported high entropy catalysts obtained in Examples 1-3 and Comparative Examples 1-7 2 Conversion rate

[0093]

[0094] 2.CO oxidation activity test

[0095] The catalysts obtained in the above examples and comparative examples were applied to CO oxidation activity tests. The activity results of the catalysts were all expressed as CO conversion rates, CO conversion rate (%) = (CO inlet - CO outlet) / CO inlet × 100%. The CO concentration was tested using MKS, and the results are shown in Table 2 below.

[0096] The conditions for the CO oxidation activity test were: the catalyst loading was 0.1 g, the reaction temperature was 50°C-300°C, the CO / O 2 (v / v=1:10), CO concentration was 1%, and the mixed gas flow rate was 300 mL / min.

[0097] Table 2 CO conversion rate of supported high entropy catalysts obtained in Examples 1-3 and Comparative Examples 1-7

[0098]

[0099] As shown in Table 1, the supported high entropy catalysts obtained in Examples 1-3 have a higher CO content than the catalysts obtained in Comparative Examples 1-7. 2It has excellent catalytic performance and stability in the hydrogenation reaction. As shown in Table 2, the supported high entropy catalysts obtained in Examples 1-3 have excellent catalytic performance in the CO oxidation reaction compared with the catalysts obtained in Comparative Examples 1-7. As shown in Table 1, the catalyst prepared in Example 1 has excellent catalytic performance in the CO oxidation reaction at 400°C. 2 The conversion rate reached 37.58%. With the further increase of temperature at 550℃, CO 2 The conversion rate reached 55.47%, and after 50h of stability test at 400℃, CO 2 The conversion rate can still reach 36.95%. As shown in Table 2, the catalyst prepared in Example 1 has a CO conversion rate of 98.24% at 300°C, and has excellent CO oxidation performance. Therefore, the supported high entropy catalyst of the present invention has excellent redox catalytic performance and stability.

[0100] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0101] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A supported high entropy catalyst, characterized in that: It includes a high entropy active component and a titanium dioxide carrier; The high entropy active component contains any four of indium, cobalt, nickel, zinc, aluminum, ruthenium and copper; The average particle size of the titanium dioxide carrier is 100nm-150nm.

2. The catalyst according to claim 1, characterized in that Based on the total amount of the high entropy active component, the copper accounts for 17.2%-23.8%; And / or, the proportion of indium is 19.1%-20.7%; And / or, the proportion of cobalt is 19.1%-20.7%; And / or, the nickel accounts for 19.1%-20.7%; And / or, the zinc accounts for 19.1%-20.7%; And / or, the proportion of ruthenium is 19.1%-20.7%.

3. The catalyst according to claim 1, characterized in that The high entropy active component contains copper, cobalt, nickel, zinc and ruthenium; Optionally, the molar ratio of copper, cobalt, nickel, zinc and ruthenium in the high entropy active component is 1:(0.8-1.2):(0.8-1.2):(0.8-1.2):(0.8-1.2).

4. The catalyst according to any one of claims 1 to 3, characterized in that Based on the mass of the titanium dioxide carrier, the mass fraction of the high entropy active component in the titanium dioxide carrier is 10%-18%; Optionally, the titanium dioxide support crystal phase is anatase.

5. A method for preparing the supported high entropy catalyst according to any one of claims 1 to 4, characterized in that: include: (1) preparing an inorganic salt precursor of a high entropy active component into a solution; (2) impregnating the solution into a titanium dioxide support and drying the support to obtain a supported high entropy catalyst precursor; (3) Reducing the supported high entropy catalyst precursor to obtain a supported high entropy catalyst.

6. The method according to claim 5, characterized in that In step (1), the inorganic salt precursor of the active component includes at least one of nitrate, sulfate or chloride.

7. The method according to claim 5, characterized in that In step (2), the drying conditions include: a temperature of 90° C. to 120° C.; and / or a drying time of 6 h to 12 h.

8. The method according to claim 5, characterized in that In step (3), the reduction treatment conditions include: a temperature of 200°C-500°C; and / or a heating rate of 3°C / min-5°C / min; and / or a time of 2h-4h.

9. A method for treating a mixed gas containing carbon monoxide and oxygen, characterized in that: A mixed gas containing carbon monoxide and oxygen is mixed with the catalyst according to any one of claims 1 to 4 or the catalyst prepared by the method according to any one of claims 5 to 8.

10. A method for treating a mixed gas containing carbon dioxide and hydrogen, characterized in that: A mixed gas containing carbon dioxide and hydrogen is mixed with the catalyst described in any one of claims 1 to 4 or the catalyst prepared by the method described in any one of claims 5 to 8.

Citation Information

Patent Citations

  • Preparation method and application of eggshell-type nickel-based catalyst

    CN103223342A

  • Low-temperature SCR denitration catalyst using carriers with different particle sizes to support Mn and preparation method thereof

    CN111450876A

  • Catalyst for catalytic combustion of organic volatile waste gas and preparation method thereof

    CN113649022A

  • High-entropy co-doped low-temperature SCR denitration catalyst as well as preparation method and application thereof

    CN113694933A

  • Ultra-dispersed high-entropy catalyst for normal-temperature hydrogenation of furfural as well as preparation method and application of ultra-dispersed high-entropy catalyst

    CN115888708A

Cited By

  • High-entropy metal oxide supported nanogold catalyst as well as preparation method and application thereof

    CN121338769A