Bimetal nano-alloy catalyst as well as preparation method and application thereof
By using bimetal nanoalloy catalysts, the problem of low selectivity for carbon-oxygen bond fracture in lignin is solved, efficient aromatic compound selectivity and cost reduction is achieved, and excessive hydrogenation of precious metal catalysts is avoided.
Patent Information
- Application Number
- CN202411375425.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to achieve selective fracture of carbon-oxygen bonds in lignin, resulting in a decrease in selectivity of aromatic compounds, and precious metal catalysts are prone to excessive hydrogenation during the fracture process, increasing costs.
Bimetal nanoalloy catalyst is used to combine precious metals and non-precious metals through a supported or encapsulated structure to reduce benzene ring adsorption, selectively activate carbon-oxygen bonds, avoid excessive hydrogenation, and improve carbon-oxygen bond fracture efficiency and selectivity of aromatic compounds.
It effectively improves the selectivity of carbon-oxygen bond breaks in lignin and its derivatives, reduces the amount of precious metals used and the cost of catalyst preparation, and improves the selectivity and conversion of aromatic compounds.
Smart Images

Figure CN118892848A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lignin conversion, and specifically relates to a bimetallic catalyst and a preparation method and application thereof. Background Art
[0002] Lignocellulosic biomass is a renewable and non-food organic material, a good alternative fuel or energy source, which is mainly composed of three highly functionalized biopolymers: cellulose, hemicellulose and lignin. Traditional lignocellulose conversion mainly utilizes the polysaccharide components in cellulose and hemicellulose, while lignin is mainly discharged as pulp waste or used as low-value-added solid fuel. Lignin accounts for 15-30% of the total weight of lignocellulose and 40% of the total energy. Therefore, whether lignin can be efficiently converted determines the economic and sustainable overall utilization of biomass. Lignin is an amorphous aromatic high molecular polymer with a three-dimensional structure. It is mainly formed by lignin monomers connected to each other through ether bonds and carbon-carbon bonds, of which carbon-oxygen bonds (mainly β-O-4) account for 60~70%. Therefore, reducing lignin and its derivatives to break their carbon-oxygen bonds to obtain aromatic compound monomers, such as phenolic compounds (4-propylguaiacol, 2,6-dimethoxyguaiacol, 4-propylphenol, guaiacol, phenol, etc.) and light aromatic hydrocarbons BTX (benzene, toluene, xylene), plays an important role in realizing the refined transformation and utilization of lignin.
[0003] During the carbon-oxygen bond cleavage of lignin and its derivatives under reducing conditions, the hydrogenation of aromatic rings to generate cycloalkane products is a competitive reaction, which reduces the selectivity of lignin monomers or aromatic compounds. Therefore, it is of great significance to provide a catalyst that can achieve the selective cleavage of carbon-oxygen bonds and thus improve the selectivity of lignin monomers or aromatic compounds. Summary of the invention
[0004] The purpose of the present invention is to provide a bimetallic nano alloy catalyst and its preparation method and application. When the bimetallic catalyst provided by the present invention is used to catalyze the reduction of lignin and its derivatives, the selective breaking of carbon-oxygen bonds can be achieved, thereby improving the selectivity of aromatic compounds.
[0005] In order to achieve the above object, the present invention provides the following technical solutions: The present invention provides a bimetallic nano alloy catalyst, the chemical composition of which includes a bimetallic nano alloy and a carrier; the bimetallic nano alloy is a nano alloy of a noble metal and a non-noble metal; The bimetallic nano alloy catalyst includes a supported bimetallic nano alloy catalyst or an encapsulated bimetallic nano alloy catalyst; The supported bimetallic nano-alloy catalyst comprises a carrier and a bimetallic nano-alloy supported on the carrier; The encapsulated bimetallic nano-alloy catalyst comprises a bimetallic nano-alloy and a carrier encapsulated on the surface of the bimetallic nano-alloy.
[0006] Preferably, the noble metal includes ruthenium, rhodium, palladium, osmium, iridium or platinum; The non-precious metals include iron, cobalt, nickel, copper, molybdenum or zinc.
[0007] Preferably, the mass percentages of the noble metal and the non-noble metal in the bimetallic nano-alloy catalyst are independently 0.1-20%.
[0008] Preferably, the carrier comprises a carbon material or a heteroatom-doped carbon material; The heteroatom in the heteroatom-doped carbon material includes one or more of nitrogen, sulfur and phosphorus; The carbon material and the carbon material in the heteroatom-doped carbon material independently include one or more of activated carbon, carbon nanotubes, graphene, hollow carbon and mesoporous carbon.
[0009] The present invention provides a method for preparing the supported bimetallic nano-alloy catalyst described in the above technical solution, comprising the following steps: The carrier is placed in a metal salt solution for impregnation-reduction to obtain a supported bimetallic nano-alloy catalyst; the metal salt in the metal salt solution includes a noble metal salt and a non-noble metal salt.
[0010] Preferably, the impregnation-reduction comprises co-impregnation-reduction or step-by-step impregnation-reduction; The co-impregnation-reduction comprises the following steps: placing the carrier in a mixed solution of a noble metal salt and a non-noble metal salt for a first impregnation followed by a first reduction; The step-by-step impregnation-reduction comprises the following steps: placing the carrier in a precious metal salt solution for a second impregnation and then a second reduction, and then placing the carrier in a non-precious metal salt solution for a third impregnation and then a third reduction; or, placing the carrier in a non-precious metal salt solution for a fourth impregnation and then a fourth reduction, and then placing the carrier in a precious metal salt solution for a fifth impregnation and then a fifth reduction.
[0011] Preferably, the first reduction, the second reduction, the third reduction, the fourth reduction and the fifth reduction independently comprise thermal reduction, wet chemical reduction or electroreduction.
[0012] Preferably, the reducing agent used in the thermal reduction includes hydrogen or a hydrogen-inert gas mixture; the temperature of the thermal reduction is 200-1200° C., and the time is 0.5-6 hours; The reducing agent used in the wet chemical reduction includes one or more of sodium borohydride, hydrazine hydrate, citric acid and ethanol; the temperature of the wet chemical reduction is 10-100° C., and the time is 0.5-6 hours; The voltage of the electroreduction is 0.05-1.5V, and the time is 0.5-2h.
[0013] The present invention provides a method for preparing the encapsulated bimetallic nano-alloy catalyst described in the above technical solution, comprising the following steps: The carrier precursor, metal salt, surfactant and water are mixed, subjected to hydrothermal reduction reaction and then heated for carbonization to obtain an encapsulated bimetallic nano alloy catalyst; the metal salt in the metal salt solution includes noble metal salt and non-noble metal salt.
[0014] The present invention provides the use of the bimetallic nanoalloy catalyst described in the above technical solution or the supported bimetallic nanoalloy catalyst prepared by the preparation method described in the above technical solution or the encapsulated bimetallic nanoalloy catalyst prepared by the preparation method described in the above technical solution in catalyzing the selective reduction of lignin substances into aromatic compounds.
[0015] Beneficial technical effects: The bimetallic nano-alloy catalyst provided by the present invention can effectively reduce the adsorption of benzene rings on metal active sites, and selectively activate the carbon-oxygen bonds between benzene rings, thereby catalyzing the selective breakage of carbon-oxygen bonds during the reduction of lignin and / or lignin derivatives. It not only avoids the excessive hydrogenation of aromatic rings during the reaction of carbon-oxygen bond breakage of lignin and / or lignin derivatives by traditional precious metal catalysts, improves the carbon-oxygen bond breakage efficiency and the selectivity of aromatic compounds, but also effectively reduces the use of precious metals and the cost of catalyst preparation.
[0016] The present invention provides a method for preparing the bimetallic nano alloy catalyst described in the above technical solution. The preparation method provided by the present invention is simple and controllable in operation, low in cost, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the catalytic reduction reaction of diphenyl ether; Figure 2 XRD patterns of Ru-Co / C bimetallic nanoalloy catalysts with different metal ratios. DETAILED DESCRIPTION
[0018] The present invention provides a bimetallic nano alloy catalyst, the chemical composition of which includes a bimetallic nano alloy and a carrier; the bimetallic nano alloy is a nano alloy of a noble metal and a non-noble metal; The bimetallic nano alloy catalyst includes a supported bimetallic nano alloy catalyst or an encapsulated bimetallic nano alloy catalyst; The supported bimetallic nano-alloy catalyst comprises a carrier and a bimetallic nano-alloy supported on the carrier; The encapsulated bimetallic nano-alloy catalyst comprises a bimetallic nano-alloy and a carrier encapsulated on the surface of the bimetallic nano-alloy.
[0019] In the present invention, unless otherwise specified, the reagents used are commercially available products well known to those skilled in the art.
[0020] In the present invention, the noble metal preferably includes ruthenium, rhodium, palladium, osmium, iridium or platinum; the mass percentage of the noble metal in the bimetallic nanoalloy catalyst is preferably 0.1-20%, more preferably 1-15%, and most preferably 5-10%.
[0021] In the present invention, the non-precious metal preferably includes iron, cobalt, nickel, copper, molybdenum or zinc; the mass percentage of the non-precious metal in the bimetallic nanoalloy catalyst is preferably 0.1-20%, more preferably 1-15%, and most preferably 5-10%.
[0022] In the present invention, the carrier preferably includes a carbon material or a heteroatom-doped carbon material; the heteroatom in the heteroatom-doped carbon material preferably includes one or more of nitrogen, sulfur and phosphorus; the carbon material and the carbon material in the heteroatom-doped carbon material independently preferably include one or more of activated carbon, carbon nanotubes, graphene, hollow carbon and mesoporous carbon. In the present invention, the molar ratio of the heteroatom to the carbon material in the heteroatom-doped carbon material is preferably 1-20%, more preferably 3-15%, and most preferably 4-10%.
[0023] The present invention provides a method for preparing the supported bimetallic nano-alloy catalyst described in the above technical solution, comprising the following steps: placing a carrier in a metal salt solution for immersion-reduction to obtain a supported bimetallic nano-alloy catalyst; the metal salt in the metal salt solution comprises a noble metal salt and a non-noble metal salt.
[0024] In the present invention, the impregnation-reduction preferably includes co-impregnation-reduction or stepwise impregnation-reduction.
[0025] In the present invention, the co-impregnation-reduction comprises the following steps: placing the carrier in a mixed solution of a noble metal salt and a non-noble metal salt for a first impregnation and then a first reduction.
[0026] In the present invention, the molar ratio of the non-precious metal to the precious metal in the mixed solution is preferably 0.1-100:1, more preferably 1-50:1, and most preferably 5-30:1; the liquid-solid ratio of the mixed solution to the carrier is preferably 5-200mL:1g, more preferably 20-100mL:1g, and most preferably 50-80mL:1g; the temperature of the first impregnation is preferably 10-30°C, more preferably 15-25°C, and most preferably 20-22°C; the time of the first impregnation is preferably 0.5-6h, more preferably 2-4h, and most preferably 3-3.5h. The present invention controls the molar ratio of the precious metal salt and the non-precious metal salt, regulates the atomic ratio of the bimetal in the bimetallic nanoalloy catalyst, reduces the amount of precious metal used while adjusting the electronic structure of the alloy, and further reduces the cost.
[0027] In the present invention, the mixed solution is preferably added dropwise; the rate of the dropwise addition is preferably 1-20 mL / min, more preferably 5-10 mL / min, and most preferably 6-8 mL / min.
[0028] After the first impregnation is completed, the present invention preferably includes first drying the first impregnated carrier obtained by the first impregnation. In the present invention, the temperature of the first drying is preferably 40-100° C., more preferably 50-80° C., and most preferably 60-70° C.; the time of the first drying is preferably 0.5-12 hours, more preferably 2-6 hours, and most preferably 3-5 hours.
[0029] In the present invention, the first reduction preferably includes thermal reduction, wet chemical reduction or electrical reduction.
[0030] In the present invention, the reducing agent used in the thermal reduction preferably includes hydrogen or a hydrogen-inert gas mixture; the volume percentage of hydrogen in the hydrogen-inert gas mixture is preferably 0.5~100%, more preferably 5~20%, and most preferably 10~15%; the flow rates of the hydrogen and the hydrogen-inert gas mixture are independently preferably 20~1000mL / min, more preferably 50~800mL / min, and most preferably 100~500mL / min; the temperature of the thermal reduction is preferably 200~1200℃, more preferably 400~1000℃, and most preferably 600~800℃; the time of the thermal reduction is preferably 0.5~6h, more preferably 1~5h, and most preferably 3~4h; the heating rate to the temperature of the thermal reduction is preferably 0.5~20℃ / min, more preferably 1~5℃ / min, and most preferably 2~3℃ / min.
[0031] In the present invention, the reducing agent used in the wet chemical reduction preferably includes one or more of sodium borohydride, hydrazine hydrate, citric acid and ethanol; the temperature of the wet chemical reduction is preferably 10~100°C, more preferably 25~100°C, and most preferably 30~50°C; the time of the wet chemical reduction is preferably 0.5~6h, more preferably 1~5h, and most preferably 3~4h.
[0032] In the present invention, the electroreduction preferably includes cathode reduction; the voltage of the electroreduction is preferably 0.05~1.5V, more preferably 0.1~1.2V, most preferably 0.5~1V; the time of the electroreduction is preferably 0.5~2h, more preferably 0.8~1.5h, most preferably 1~1.2h.
[0033] After the first reduction is completed, the present invention preferably further includes subjecting the first reduction product obtained by the first reduction to a first passivation. In the present invention, the passivating agent used in the first passivation is preferably an oxygen-inert gas mixture, more preferably an oxygen-argon gas mixture; the volume percentage of oxygen in the oxygen-inert gas mixture is preferably 0.1-5%, more preferably 0.5-2%, and most preferably 1-1.5%; the time of the first passivation is preferably 10-120 min, more preferably 30-60 min, and most preferably 40-50 min. The present invention passivates the reduction product and purges a large amount of hydrogen adsorbed on the surface of the bimetallic alloy, thereby avoiding metal combustion caused by direct exposure of the product to the air; moreover, the oxygen content used for passivation is low and less than the oxygen content in the air, the surface oxidation of the metal does not reach the level of forming metal oxides, and the effect on the catalyst performance is small, and the catalyst is used for catalytic reaction at high temperature and high hydrogen pressure, which also has a certain reduction effect on the catalyst.
[0034] In the present invention, the step-by-step impregnation-reduction comprises the following steps: placing the carrier in a precious metal salt solution for a second impregnation and then a second reduction, and then placing the carrier in a non-precious metal salt solution for a third impregnation and then a third reduction; or, placing the carrier in a non-precious metal salt solution for a fourth impregnation and then a fourth reduction, and then placing the carrier in a precious metal salt solution for a fifth impregnation and then a fifth reduction.
[0035] In the present invention, the carrier is placed in a noble metal salt solution for a second impregnation and then a second reduction, and then placed in a non-noble metal salt solution for a third impregnation and then a third reduction.
[0036] In the present invention, the molar ratio of the non-precious metal in the non-precious metal salt solution to the precious metal in the precious metal salt solution is preferably 0.1-100:1, more preferably 1-50:1, and most preferably 5-30:1; the liquid-solid ratio of the precious metal salt solution to the carrier is preferably 5-200mL:1g, more preferably 20-100mL:1g, and most preferably 50-80mL:1g. In the present invention, the temperature and time of the second and third impregnations are preferably the same as those of the first impregnation, and will not be repeated here.
[0037] After the second impregnation is completed, the present invention preferably includes subjecting the second impregnated carrier obtained by the second impregnation to a second drying. After the third impregnation is completed, the present invention preferably includes subjecting the third impregnated carrier obtained by the third impregnation to a third drying. In the present invention, the temperature and time of the second drying and the third drying are preferably the same as those of the first drying, which will not be described in detail herein.
[0038] In the present invention, the noble metal salt solution is preferably added dropwise; the rate of the addition is preferably 1-20 mL / min, more preferably 5-10 mL / min, and most preferably 6-8 mL / min; the non-noble metal salt solution is preferably added dropwise; the rate of the addition is preferably 1-20 mL / min, more preferably 5-10 mL / min, and most preferably 6-8 mL / min.
[0039] In the present invention, the methods and conditions of the second reduction and the third reduction are preferably the same as those of the first reduction, and will not be described in detail herein.
[0040] After the second reduction is completed, the present invention preferably further comprises subjecting the second reduction product obtained by the second reduction to a second passivation. After the third reduction is completed, the present invention preferably further comprises subjecting the third reduction product obtained by the third reduction to a third passivation. In the present invention, the passivating agent and the passivation time used in the second passivation and the third passivation are preferably the same as those of the first passivation, and are not described in detail herein.
[0041] In the present invention, the carrier is placed in a non-noble metal salt solution for a fourth impregnation and then a fourth reduction, and then placed in a noble metal salt solution for a fifth impregnation and then a fifth reduction.
[0042] In the present invention, the molar ratio of the non-precious metal in the non-precious metal salt solution to the precious metal in the precious metal salt solution is preferably 0.1-100:1, more preferably 1-50:1, and most preferably 5-30:1; the liquid-solid ratio of the non-precious metal salt solution to the carrier is preferably 5-200mL:1g, more preferably 20-100mL:1g, and most preferably 50-80mL:1g. In the present invention, the temperature and time of the fourth and fifth impregnations are the same as those of the first impregnation, and are not repeated here.
[0043] After the fourth impregnation is completed, the present invention preferably includes subjecting the fourth impregnated carrier obtained by the fourth impregnation to a fourth drying. After the fifth impregnation is completed, the present invention preferably includes subjecting the fifth impregnated carrier obtained by the fifth impregnation to a fifth drying. In the present invention, the temperature and time of the fourth drying and the fifth drying are preferably the same as those of the first drying, which will not be described in detail herein.
[0044] In the present invention, the method of adding the non-precious metal salt solution and the precious metal salt solution and the rate of dripping are preferably the same as described above and will not be described in detail herein.
[0045] In the present invention, the manner and conditions of the fourth reduction and the fifth reduction are preferably the same as those of the first reduction, and will not be described in detail herein.
[0046] After the fourth reduction is completed, the present invention preferably further comprises subjecting the fourth reduction product obtained by the fourth reduction to a fourth passivation. After the fifth reduction is completed, the present invention preferably further comprises subjecting the fifth reduction product obtained by the fifth reduction to a fifth passivation. In the present invention, the passivating agent and the passivation time used in the fourth passivation and the fifth passivation are preferably the same as those of the first passivation, and are not described in detail herein.
[0047] The present invention provides a method for preparing an encapsulated bimetallic nano-alloy catalyst according to the above technical solution, comprising the following steps: mixing a carrier precursor, a metal salt, a surfactant and water, performing a hydrothermal reduction reaction and then heating and carbonizing to obtain an encapsulated bimetallic nano-alloy catalyst; the metal salt in the metal salt solution comprises a noble metal salt and a non-noble metal salt.
[0048] In the present invention, the hydrothermal reduction reaction preferably includes a co-hydrothermal reduction reaction or a stepwise hydrothermal reduction reaction.
[0049] In the present invention, the co-hydrothermal reduction reaction comprises the following steps: mixing a carrier precursor, a noble metal salt, a non-noble metal salt, a surfactant and water, performing a first hydrothermal reduction reaction and then a first thermal carbonization.
[0050] In the present invention, the carrier precursor preferably includes a precursor A and a precursor B; the precursor A preferably includes an aromatic compound containing at least one carboxyl group and one hydroxyl group; the aromatic compound containing at least one carboxyl group and one hydroxyl group preferably includes o-hydroxybenzoic acid and / or 2,4-dihydroxybenzoic acid; the precursor B preferably includes an aldehyde-containing organic matter or a compound that decomposes to produce formaldehyde; the aldehyde-containing organic matter preferably includes an aliphatic aldehyde compound and / or an aromatic aldehyde compound; the aliphatic aldehyde compound preferably includes one or more of formaldehyde, acetaldehyde and isobutyraldehyde; the aromatic aldehyde compound preferably includes one or more of benzaldehyde, cinnamaldehyde and vanillin; the compound that decomposes to produce formaldehyde preferably includes hexamethylenetetrammonium; the molar ratio of the precursor A to the precursor B is preferably 1:1~6, more preferably 1:2~3, and most preferably 1:2.2~2.5.
[0051] In the present invention, the surfactant preferably includes a triblock polymer, and the ratio of the hydrophilic segment to the hydrophobic segment in the triblock polymer is preferably 0.1-2:1, more preferably 0.5-1.5:1, and most preferably 1-1.2:1; the molar ratio of the surfactant to the non-precious metal in the non-precious metal salt is preferably 1:1-100, more preferably 1:3-50, and most preferably 1:5-35; the molar ratio of the surfactant to the noble metal in the noble metal salt is preferably 0.05-20:1, more preferably 0.1-10:1, and most preferably 0.5-5:1.
[0052] In the present invention, the temperature of the first hydrothermal reduction reaction is preferably 80-200°C, more preferably 140-180°C, and most preferably 160-170°C; the time of the first hydrothermal reduction reaction is preferably 1-12h, more preferably 2-6h, and most preferably 3-5h.
[0053] In the present invention, the first thermal carbonization is preferably carried out in a hydrogen-inert gas mixture; the volume percentage of hydrogen in the hydrogen-inert gas mixture is preferably 0.5~100%, more preferably 5~20%, and most preferably 10~15%; the flow rate of the hydrogen-inert gas mixture is preferably 20~1000mL / min, more preferably 50~800mL / min, and most preferably 100~500mL / min; the temperature of the first thermal carbonization is preferably 200~1200℃, more preferably 400~1000℃, and most preferably 600~800℃; the time of the first thermal carbonization is preferably 0.5~6h, more preferably 1~5h, and most preferably 3~4h; the heating rate to the temperature of the first thermal carbonization is preferably 0.5~20℃ / min, more preferably 1~5℃ / min, and most preferably 2~3℃ / min.
[0054] The present invention utilizes the binding effect between the terminal hydroxyl group of the carrier precursor and the metal cation, and obtains the encapsulated bimetallic nano alloy catalyst by self-assembly under hydrothermal reaction conditions and then heating and carbonization.
[0055] In the present invention, the step-by-step hydrothermal reduction reaction includes the following steps: mixing a carrier precursor, a noble metal salt, a surfactant and water, performing a second hydrothermal reduction reaction to obtain a first single metal catalyst solution, then performing a first thermal mixing with a non-noble metal salt and ammonia water, and performing a second thermal carbonization, or, mixing a carrier precursor, a non-noble metal salt, a surfactant and water, performing a third hydrothermal reduction reaction to obtain a second single metal catalyst solution, then performing a second thermal mixing with a noble metal salt and ammonia water, and performing a third thermal carbonization.
[0056] The present invention mixes a carrier precursor, a noble metal salt, a surfactant and water, performs a second hydrothermal reduction reaction, obtains a first single metal catalyst solution, and then performs a first thermal mixing with a non-noble metal salt and ammonia water, and performs a second thermal carbonization.
[0057] In the present invention, the carrier precursor preferably includes a precursor A and a precursor B; the precursor A preferably includes an aromatic compound containing at least one carboxyl group and one hydroxyl group; the aromatic compound containing at least one carboxyl group and one hydroxyl group preferably includes o-hydroxybenzoic acid and / or 2,4-dihydroxybenzoic acid; the precursor B preferably includes an aldehyde-containing organic matter or a compound that decomposes to produce formaldehyde; the aldehyde-containing organic matter preferably includes an aliphatic aldehyde compound and / or an aromatic aldehyde compound; the aliphatic aldehyde compound preferably includes one or more of formaldehyde, acetaldehyde and isobutyraldehyde; the aromatic aldehyde compound preferably includes one or more of benzaldehyde, cinnamaldehyde and vanillin; the compound that decomposes to produce formaldehyde preferably includes hexamethylenetetrammonium; the molar ratio of the precursor A to the precursor B is preferably 1:1~6, more preferably 1:2~3, and most preferably 1:2.2~2.5.
[0058] In the present invention, the surfactant preferably includes a triblock polymer, and the ratio of the hydrophilic segment to the hydrophobic segment in the triblock polymer is preferably 0.1-2:1, more preferably 0.5-1.5:1, and most preferably 1-1.2:1; the molar ratio of the surfactant to the noble metal in the noble metal salt is preferably 0.05-20:1, more preferably 0.1-10:1, and most preferably 0.5-5:1.
[0059] In the present invention, the temperature of the second hydrothermal reduction reaction is preferably 80-200°C, more preferably 140-180°C, and most preferably 160-170°C; the time of the second hydrothermal reduction reaction is preferably 1-12h, more preferably 2-6h, and most preferably 3-5h. In the present invention, the second thermal carbonization is preferably carried out in a hydrogen-inert gas mixture; the volume percentage of hydrogen in the hydrogen-inert gas mixture is preferably 0.5-100%, more preferably 5-20%, and most preferably 10-15%; the flow rate of the hydrogen-inert gas mixture is preferably 20-1000mL / min, more preferably 50-800mL / min, and most preferably 100-500mL / min.
[0060] In the present invention, the volume ratio of the aqueous ammonia to the first single metal catalyst solution is preferably 0.01 to 1, more preferably 0.05 to 0.5, and most preferably 0.1 to 0.25.
[0061] In the present invention, the temperature of the first thermal mixing is preferably 30-100° C., more preferably 40-80° C., most preferably 45-60° C.; the time of the first thermal mixing is preferably 1-8 h, more preferably 2-6 h, most preferably 3-4 h.
[0062] In the present invention, the temperature of the second thermal carbonization is preferably 200~1200°C, more preferably 400~1000°C, and most preferably 600~800°C; the time of the second thermal carbonization is preferably 0.5~6h, more preferably 1~5h, and most preferably 3~4h; the heating rate to the temperature of the second thermal carbonization is preferably 0.5~20°C / min, more preferably 1~5°C / min, and most preferably 2~3°C / min.
[0063] The invention utilizes the thermal diffusion phenomenon of metal salts in the reduction process to prepare encapsulated bimetallic nano alloy catalysts in steps.
[0064] The present invention mixes a carrier precursor, a non-precious metal salt, a surfactant and water, performs a third hydrothermal reduction reaction, obtains a second monometallic catalyst solution, and then performs a second thermal mixing with a precious metal salt and ammonia water, and performs a third thermal carbonization.
[0065] In the present invention, the carrier precursor preferably includes a precursor A and a precursor B; the precursor A preferably includes an aromatic compound containing at least one carboxyl group and one hydroxyl group; the aromatic compound containing at least one carboxyl group and one hydroxyl group preferably includes o-hydroxybenzoic acid and / or 2,4-dihydroxybenzoic acid; the precursor B preferably includes an aldehyde-containing organic matter or a compound that decomposes to produce formaldehyde; the aldehyde-containing organic matter preferably includes an aliphatic aldehyde compound and / or an aromatic aldehyde compound; the aliphatic aldehyde compound preferably includes one or more of formaldehyde, acetaldehyde and isobutyraldehyde; the aromatic aldehyde compound preferably includes one or more of benzaldehyde, cinnamaldehyde and vanillin; the compound that decomposes to produce formaldehyde preferably includes hexamethylenetetrammonium; the molar ratio of the precursor A to the precursor B is preferably 1:1~6, more preferably 1:2~3, and most preferably 1:2.2~2.5.
[0066] In the present invention, the surfactant preferably includes a triblock polymer, and the ratio of the hydrophilic segment to the hydrophobic segment in the triblock polymer is preferably 0.1-2:1, more preferably 0.5-1.5:1, and most preferably 1-1.2:1; the molar ratio of the surfactant to the non-precious metal in the non-precious metal salt is preferably 1:1-100, more preferably 1:3-50, and most preferably 1:5-35.
[0067] In the present invention, the temperature of the third hydrothermal reduction reaction is preferably 80-200°C, more preferably 140-180°C, and most preferably 160-170°C; the time of the third hydrothermal reduction reaction is preferably 1-12h, more preferably 2-6h, and most preferably 3-5h.
[0068] In the present invention, the third thermal carbonization is preferably carried out in a hydrogen-inert gas mixture; the volume percentage of hydrogen in the hydrogen-inert gas mixture is preferably 0.5~100%, more preferably 5~20%, most preferably 10~15%; the flow rate of the hydrogen-inert gas mixture is preferably 20~1000mL / min, more preferably 50~800mL / min, most preferably 100~500mL / min.
[0069] In the present invention, the volume ratio of the aqueous ammonia to the second single metal catalyst solution is preferably 0.01 to 1, more preferably 0.05 to 0.5, and most preferably 0.1 to 0.25.
[0070] In the present invention, the temperature of the second thermal mixing is preferably 30-100° C., more preferably 40-80° C., most preferably 45-60° C.; the time of the second thermal mixing is preferably 1-8 h, more preferably 2-6 h, most preferably 3-4 h.
[0071] In the present invention, the temperature of the third thermal carbonization is preferably 200~1200°C, more preferably 400~1000°C, and most preferably 600~800°C; the time of the third thermal carbonization is preferably 0.5~6h, more preferably 1~5h, and most preferably 3~4h; the heating rate to the temperature of the third thermal carbonization is preferably 0.5~20°C / min, more preferably 1~5°C / min, and most preferably 2~3°C / min.
[0072] The present invention provides the use of the bimetallic nanoalloy catalyst described in the above technical solution or the bimetallic nanoalloy catalyst prepared by the preparation method described in the above technical solution in catalyzing the selective reduction of lignin-like substances to aromatic compounds. When the bimetallic nanoalloy catalyst provided by the present invention is used to catalyze the selective reduction of lignin-like substances to aromatic compounds, it can effectively reduce the adsorption of benzene rings on metal active sites, and selectively activate the carbon-oxygen bonds between benzene rings, thereby catalyzing the selective breakage of carbon-oxygen bonds during the reduction of lignin and / or lignin derivatives, which not only avoids the excessive hydrogenation of aromatic rings during the reaction of carbon-oxygen bond breakage of lignin and / or lignin derivatives by traditional precious metal catalysts, improves the efficiency of carbon-oxygen bond breakage and the selectivity of aromatic compounds, but also effectively reduces the use of precious metals and the cost of catalyst preparation.
[0073] In the present invention, the lignin-like substances are preferably derived from birch, poplar or straw; the lignin-like substances preferably include lignin and / or lignin derivatives; the lignin derivatives preferably include lignin polymers and / or lignin dimers; the lignin dimers include one or more of phenyl benzyl ether, phenyl phenethyl ether and diphenyl ether.
[0074] In the present invention, the aromatic compound preferably includes phenolic compounds and / or light aromatic hydrocarbons (BTX); the phenolic compound preferably includes one or more of 4-propylguaiacol, 2,6-dimethoxyguaiacol, 4-propylphenol, guaiacol and phenol; the light aromatic hydrocarbon preferably includes one or more of benzene, toluene and xylene.
[0075] In the present invention, the mass ratio of the bimetallic nano alloy catalyst to the lignin-based substance is preferably 1:10-1000, more preferably 1:100-800, and more preferably 1:400-500.
[0076] In all the embodiments and comparative examples provided by the present invention, the conditions for gas phase-mass spectrometry detection are as follows: gas phase conditions: the chromatographic column is a 624-UI capillary column, 30m×0.53mm×3µm; the temperature of the chromatographic column is programmed temperature rise, and the program of the programmed temperature rise is: 0~20min, 40℃, 20~40℃, heating to 200℃ at a rate of 10℃ / min, 40~60min, 200℃; the total flow rate of the injection port is 35mL / min, the split ratio is 5:1, and the injection port temperature is 250℃; the detector is FID, 240℃, the hydrogen flow rate is 30mL / min, the air flow rate is 400mL / min, and the tail nitrogen flow rate is 35mL / min.
[0077] Example 1 1.2mmol 2,4-dihydroxybenzoic acid, 0.5mmol hexamethylenetetraammonium, 0.24mmol SO (sodium oleate), 0.0075mmol triblock polymer P123 and 3mol RuCl3 were dissolved in 80mL deionized water, transferred to a reactor, and placed in an oven at 160℃ for 4h. After the reaction, the reactor was cooled to room temperature, the reaction product was centrifuged and vacuum dried at 60℃ for 8h. The dried sample was placed in a tube furnace, heated to 300℃ at a rate of 2℃ / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 2h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% was introduced for passivation for 0.5h to obtain a precursor of hollow carbon sphere encapsulated Ru, which was recorded as Ru / C precursor.
[0078] Under stirring conditions, a 3 mol / L Co(NO3)2 solution was added dropwise to the Ru / C precursor obtained in the previous step. After the addition was completed, the mixture was stirred for 4 h at room temperature, and then transferred to a vacuum drying oven and dried at 60°C for 8 h. The dried sample was placed in a tube furnace, heated to 500°C at a rate of 2°C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% hydrogen was introduced for thermal reduction for 2 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% oxygen was introduced for passivation for 0.5 h to obtain a Ru-Co / C bimetallic nanoalloy catalyst. The molar ratio of Ru element in RuCl3 solution to Co element in Co(NO3)2 solution was 1:3.
[0079] Example 2 The Ru-Co / C bimetallic nanoalloy catalyst was prepared by the preparation method provided in Example 1, and the only difference from Example 1 was that the molar ratio of the Ru element in the RuCl3 solution to the Co element in the Co(NO3)2 solution was 1:4.
[0080] Example 3 The Ru-Co / C bimetallic nanoalloy catalyst was prepared by the preparation method provided in Example 1, and the only difference from Example 1 was that the molar ratio of the Ru element in the RuCl3 solution to the Co element in the Co(NO3)2 solution was 1:5.
[0081] 30 mg of the Ru-Co / C bimetallic nanoalloy catalyst prepared in Examples 1 to 3 and the commercial Ru / C catalyst (Ru / C, sigma) were added to a high-temperature and high-pressure reactor containing 5 mL of isopropanol and 1 mmol of diphenyl ether, and hydrogen gas at a pressure of 2 MPa was introduced. The temperature was raised to 200°C for a reduction reaction for 3 h. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with isopropanol, the rinse liquid was collected, and dodecane was added as an internal standard. The rinse liquid was qualitatively and quantitatively analyzed by gas phase-mass spectrometry. The results are shown in Tables 1 and Figure 1 shown.
[0082] Table 1 Conversion rate and selectivity of Ru-Co / C bimetallic nanoalloy catalysts prepared in Examples 1 to 3 and commercial Ru / C catalysts
[0083] Figure 1 is a schematic diagram of the catalytic reduction reaction of diphenyl ether, and Table 1 shows the conversion rate and selectivity of the Ru-Co / C bimetallic nano alloy catalyst and the commercial Ru / C catalyst prepared in Examples 1 to 3. Figure 1 As shown in Table 1, the Ru-Co / C bimetallic nano-alloy catalyst provided by the present invention has high selectivity and yield for the selective reduction of diphenyl ether.
[0084] Figure 2 The XRD patterns of the Ru-Co / C bimetallic nano-alloy catalyst and the commercial Ru / C catalyst are shown in Figure 1, Example 2, Example 3 and the commercial Ru / C catalyst from top to bottom. Figure 2 It can be seen that the structure of the bimetallic material changes with the molar ratio of the two metals. As the amount of Co doping gradually increases, it transforms from the RuCo alloy phase to the Ru-doped Co phase.
[0085] Example 4 Under stirring conditions, 10 μL of 10 mol / L K2PdCl4 solution was added dropwise to 100 mg of carbon support. After the addition was completed, stirring was continued at room temperature for 2 h, and then the sample was transferred to a vacuum drying oven and dried at 60 ° C for 8 h. The dried sample was placed in a tube furnace, heated to 300 ° C at a rate of 2 ° C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% hydrogen was introduced for thermal reduction for 0.5 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% oxygen was introduced for passivation for 0.5 h to obtain a Pd / C precursor.
[0086] Under stirring conditions, 100µL of 10mol / L FeCl3 solution was added dropwise to the Pd / / C precursor obtained in the previous step. After the addition was completed, stirring was continued at room temperature for 2h, and then the sample was transferred to a vacuum drying oven and dried at 60°C for 8h. The dried sample was placed in a tube furnace, heated to 500°C at a rate of 2°C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 1h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5h to obtain a Pd-Fe / C bimetallic nanoalloy catalyst.
[0087] 30 mg of the prepared Pd-Fe / C bimetallic nanoalloy catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of methanol and 1 mmol of 1-(3,4-dimethoxyphenyl)-2-(2-methoxyphenyl)-propane-1,3-diol (Veratrylglycerol-beta-guaiacylether, VG), and hydrogen gas at a pressure of 2 MPa was introduced, and the temperature was raised to 200 ° C for reduction reaction for 3 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas chromatography-mass spectrometry.
[0088] The conversion rate of VG reduced to aromatic ring compound monomers by the Pd-Fe / C bimetallic nano-alloy catalyst prepared in this example was 100%, and the yield of aromatic ring compound monomers was 90%.
[0089] Example 5 Under stirring conditions, 20µL of 10mol / L K2PtCl6 solution was added dropwise to 100mg of activated carbon carrier. After the addition was completed, stirring was continued at room temperature for 2h, and then transferred to a vacuum drying oven and dried at 60℃ for 8h. The dried sample was dispersed in 20mL of deionized water, placed in an ice water bath after ultrasonic treatment for a period of time, and 10mL of 1mol / L sodium borohydride aqueous solution was added dropwise under stirring conditions. After the addition was completed, the reduction reaction was carried out at room temperature and stirring for 2h. After the reaction was completed, the obtained reaction liquid was centrifuged, and the obtained solid product was transferred to a vacuum drying oven and dried at 60℃ for 8h to obtain a Pt / C precursor.
[0090] Under stirring conditions, 1 mL of 10 mol / L Co(NO3)2 solution was added dropwise to the Pt / C precursor obtained in the previous step. After the addition was completed, stirring was continued at room temperature for 2 h, and then the sample was transferred to a vacuum drying oven and dried at 60°C for 8 h. The dried sample was placed in a tube furnace, heated to 500°C at a rate of 2°C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 1 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5 h to obtain a Pt-Co / C bimetallic nanoalloy catalyst.
[0091] 30 mg of the prepared Pt-Co / C bimetallic nanoalloy catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of methanol and 1 mmol of poplar lignin, and hydrogen at a pressure of 2 MPa was introduced, and the temperature was raised to 200 ° C for reduction reaction for 12 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas phase-mass spectrometry.
[0092] The conversion rate of the Pt-Co / C bimetallic nano-alloy catalyst prepared in this example in reducing poplar lignin to lignin monomer was 85%, and the yield of aromatic ring compound monomer was 80%.
[0093] Example 6 Under stirring conditions, 10 µL of 10 mol / L RuCl3 solution was added dropwise to 100 mg of activated carbon support. After the addition was completed, stirring was continued at room temperature for 2 h, and then transferred to a vacuum drying oven and dried at 60 ° C for 8 h. The dried sample was dispersed in 20 mL of ethylene glycol, and after ultrasonication for a period of time, refluxed at 80 ° C for 4 h. After the reaction was completed, the obtained reaction liquid was centrifuged, and the obtained solid product was washed with ethanol 3 times and transferred to a vacuum drying oven, and dried at 60 ° C for 8 h to obtain a Ru / C precursor.
[0094] Under stirring conditions, 1 mL of 10 mol / L Ni(NO3)2 solution was added dropwise to the Ru / C precursor obtained in the previous step. After the addition was completed, stirring was continued at room temperature for 2 h, and then the sample was transferred to a vacuum drying oven and dried at 60°C for 8 h. The dried sample was placed in a tube furnace, heated to 500°C at a rate of 2°C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 1 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5 h to obtain a Ru-Ni / C bimetallic nanoalloy catalyst.
[0095] 30 mg of the prepared Ru-Ni / C bimetallic nanoalloy catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of water and 1 mmol of 2-methoxy(2'-methyl-2'-phenylethyl)phenyl ether, and hydrogen gas at a pressure of 2 MPa was introduced, and the temperature was raised to 200°C for a reduction reaction for 4 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas chromatography-mass spectrometry.
[0096] The conversion rate of the Ru-Ni / C bimetallic nanoalloy catalyst prepared in this example in reducing 2-methoxy(2'-methyl-2'-phenylethyl)phenyl ether to aromatic ring compound monomers was 100%, and the yield of aromatic ring compound monomers was 95%.
[0097] Example 7 Under stirring conditions, 10 mL of a mixed solution containing 3 mol / L RuCl3 and 3 mol / L Co(NO3)2 was added dropwise to 100 mg of the carbon support. After the addition was completed, stirring was continued at room temperature for 4 h, and then the sample was transferred to a vacuum drying oven and dried at 60 ° C for 8 h. The dried sample was placed in a tube furnace, heated to 500 ° C at a rate of 2 ° C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 2 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5 h to obtain a Ru-Co / C bimetallic nanoalloy catalyst.
[0098] 30 mg of the prepared Ru-Co / C bimetallic nanoalloy catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of isopropanol and 1 mmol of diphenyl ether, and hydrogen gas at a pressure of 2 MPa was introduced, and the temperature was raised to 200°C for a reduction reaction for 3 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas chromatography-mass spectrometry.
[0099] The conversion rate of diphenyl ether reduced to aromatic ring compound monomers by the Ru-Co / C bimetallic nano-alloy catalyst prepared in this comparative example was 100%, and the yield of the aromatic ring compound monomers was 70%.
[0100] Comparative Example 1 Under stirring conditions, 10 mL of a 3 mol / L RuCl3 solution was added dropwise to 100 mg of the carbon support. After the addition was completed, stirring was continued at room temperature for 4 h, and then the sample was transferred to a vacuum drying oven and dried at 60 ° C for 8 h. The dried sample was placed in a tube furnace, heated to 500 ° C at a rate of 2 ° C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 2 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5 h to obtain a Ru / C single metal catalyst.
[0101] 30 mg of the prepared Ru / C monometallic catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of isopropanol and 1 mmol of diphenyl ether, and hydrogen gas at a pressure of 2 MPa was introduced, and the temperature was raised to 200°C for a reduction reaction for 3 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas chromatography-mass spectrometry.
[0102] The conversion rate of diphenyl ether reduced to aromatic ring compound monomers by the Ru / C single metal catalyst prepared in this comparative example was 100%, and the yield of aromatic ring compound monomers was 9.7%.
[0103] Comparative Example 2 Under stirring conditions, 10 mL of a 3 mol / L Co(NO3)2 solution was added dropwise to 100 mg of the carbon support. After the addition was completed, stirring was continued at room temperature for 4 h, and then the sample was transferred to a vacuum drying oven and dried at 60 °C for 8 h. The dried sample was placed in a tube furnace, heated to 500 °C at a rate of 2 °C / min, and a hydrogen-argon mixed gas with a volume percentage of 10% of hydrogen was introduced for thermal reduction treatment for 2 h. After the thermal reduction was completed, the tube furnace was cooled to room temperature, and an oxygen-argon mixed gas with a volume percentage of 0.5% of oxygen was introduced for passivation for 0.5 h to obtain a Co / C single metal catalyst.
[0104] 30 mg of the prepared Co / C monometallic catalyst was added to a high-temperature and high-pressure reactor containing 5 mL of isopropanol and 1 mmol of diphenyl ether, and hydrogen gas at a pressure of 2 MPa was introduced, and the temperature was raised to 200°C for a reduction reaction for 3 hours. After the reaction was completed, the reactor was cooled to room temperature, the inner wall of the reactor was rinsed with a large amount of solvent, the rinse liquid was collected, and dodecane was added as an internal standard, and the rinse liquid was qualitatively and quantitatively analyzed by gas chromatography-mass spectrometry.
[0105] The conversion rate of diphenyl ether reduced to aromatic ring compound monomers by the Co / C single metal catalyst prepared in this comparative example was 0%, and the yield of aromatic ring compound monomers was 0%.
[0106] In summary, the bimetallic nano-alloy catalyst provided by the present invention can catalyze the selective breaking of carbon-oxygen bonds in lignin and its derivatives, thereby improving the selectivity of aromatic ring compound monomers and / or lignin monomers.
[0107] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A bimetallic nanoalloy catalyst, the chemical composition of which includes a bimetallic nanoalloy and a carrier; the bimetallic nanoalloy is a nanoalloy of a noble metal and a non-noble metal; The bimetallic nano alloy catalyst includes a supported bimetallic nano alloy catalyst or an encapsulated bimetallic nano alloy catalyst; The supported bimetallic nano-alloy catalyst comprises a carrier and a bimetallic nano-alloy supported on the carrier; The encapsulated bimetallic nano-alloy catalyst comprises a bimetallic nano-alloy and a carrier encapsulated on the surface of the bimetallic nano-alloy.
2. The bimetallic nano alloy catalyst according to claim 1, characterized in that: The noble metal includes ruthenium, rhodium, palladium, osmium, iridium or platinum; The non-precious metals include iron, cobalt, nickel, copper, molybdenum or zinc.
3. The bimetallic nano alloy catalyst according to claim 1 or 2, characterized in that: The mass percentages of the noble metal and the non-noble metal in the bimetallic nano alloy catalyst are independently 0.1-20%.
4. The bimetallic nano alloy catalyst according to claim 1, characterized in that: The carrier comprises a carbon material or a heteroatom-doped carbon material; The heteroatom in the heteroatom-doped carbon material includes one or more of nitrogen, sulfur and phosphorus; The carbon material and the carbon material in the heteroatom-doped carbon material independently include one or more of activated carbon, carbon nanotubes, graphene, hollow carbon and mesoporous carbon.
5. The method for preparing the supported bimetallic nano alloy catalyst according to any one of claims 1 to 4, characterized in that: The following steps are involved: The carrier is placed in a metal salt solution for impregnation-reduction to obtain a supported bimetallic nano-alloy catalyst; The metal salt in the metal salt solution includes noble metal salts and non-noble metal salts.
6. The preparation method according to claim 5, characterized in that: The impregnation-reduction includes co-impregnation-reduction or step-by-step impregnation-reduction; The co-impregnation-reduction comprises the following steps: placing the carrier in a mixed solution of a noble metal salt and a non-noble metal salt for a first impregnation followed by a first reduction; The step-by-step impregnation-reduction comprises the following steps: placing the carrier in a precious metal salt solution for a second impregnation and then a second reduction, and then placing the carrier in a non-precious metal salt solution for a third impregnation and then a third reduction; or, placing the carrier in a non-precious metal salt solution for a fourth impregnation and then a fourth reduction, and then placing the carrier in a precious metal salt solution for a fifth impregnation and then a fifth reduction.
7. The preparation method according to claim 6, characterized in that: The first reduction, the second reduction, the third reduction, the fourth reduction and the fifth reduction independently comprise thermal reduction, wet chemical reduction or electrical reduction.
8. The preparation method according to claim 7, characterized in that: The reducing agent used in the thermal reduction includes hydrogen or a hydrogen-inert gas mixture; the temperature of the thermal reduction is 200-1200° C., and the time is 0.5-6 hours; The reducing agent used in the wet chemical reduction includes one or more of sodium borohydride, hydrazine hydrate, citric acid and ethanol; the temperature of the wet chemical reduction is 10-100° C., and the time is 0.5-6 hours; The voltage of the electroreduction is 0.05-1.5V, and the time is 0.5-2h.
9. The method for preparing the encapsulated bimetallic nano alloy catalyst according to any one of claims 1 to 4, characterized in that: The following steps are involved: The carrier precursor, metal salt, surfactant and water are mixed, subjected to hydrothermal reduction reaction and then heated for carbonization to obtain an encapsulated bimetallic nano alloy catalyst; the metal salt in the metal salt solution includes noble metal salt and non-noble metal salt.
10. Use of the bimetallic nanoalloy catalyst according to any one of claims 1 to 4, the supported bimetallic nanoalloy catalyst prepared by the preparation method according to any one of claims 5 to 8, or the encapsulated bimetallic nanoalloy catalyst prepared by the preparation method according to claim 9 in catalyzing the selective reduction of lignin substances to aromatic compounds.
Citation Information
Patent Citations
Method for preparing aromatic hydrocarbon by carrying out catalytic hydrodeoxygenation on lignin
CN104744204A
Preparation method of carbon-coated cobalt-silver alloy catalyst
CN110479306A
Method for hydrogenolysis of lignin into aromatic hydrocarbon by using palladium alloy catalyst
CN114073964A
Supported diatomic catalyst as well as preparation method and application thereof
CN116116433A
Ruthenium-non-noble metal alloy catalyst and preparation method thereof
CN116479298A