Column-machine combined process for recycling zinc metal in lead-zinc flotation tailings

Through the combined process of column machine, the combination of CPT flotation column and JJF flotation machine is used to optimize the capture of fine-grained and coarse-grained minerals, which solves the problem of low zinc metal recovery in flotation tailings, and achieves a short process. Recycling effect of zinc metal with low cost and good flotation index.

CN118892911AActive Publication Date: 2024-11-05NORTHWEST RES INST OF MINING & METALLURGY INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411211179.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-05
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the existing ore dressing process, the zinc metal recovery rate in flotation tailings is relatively low, the process is complex and the cost is high, making it difficult to take into account the grade and recovery rate of zinc concentrate.

Method used

Using the combined process of column machine, the CPT flotation column and the JJF flotation machine are used to perform pre-enrichment and re-frigeration and selection, and the micro-bubble foaming device and JJF flotation are respectively used to perform pre-enrichment and re-frigeration and selection. The stirring strength of the machine is optimized for the capture of fine and coarse grade minerals, and the recovery of zinc metals with short processes and low costs.

Benefits of technology

It improves the grade and recovery rate of zinc concentrate, simplifies the process, reduces economic costs, and has excellent flotation indicators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892911A_ABST
    Figure CN118892911A_ABST
Patent Text Reader

Abstract

The invention relates to a column-machine combined process for recycling zinc metal in lead-zinc flotation tailings, which comprises the following steps of: (1) carrying out size mixing on the lead-zinc flotation tailings with a zinc metal recycling value to obtain an ore feeding product; (2) a CPT flotation column is adopted for conducting zinc primary roughing on the feeding product, and primary roughing concentrate and primary roughing tailings are obtained; (3) the primary roughing tailings are graded, and fine-fraction products with the particle size being-0.074 mm and coarse-fraction products with the particle size being + 0.074 mm are obtained; (4) carrying out secondary roughing on the coarse fraction product by adopting a JJF flotation machine to obtain secondary roughing concentrate and secondary roughing tailings; (5) re-grinding the secondary roughing concentrate to obtain re-ground ore pulp; (6) the primary roughing concentrate and the reground ore pulp are combined and then subjected to concentration through a CPT flotation column, and zinc concentrate and concentrated middlings are obtained; and (7) scavenging the secondary roughing tailings by adopting a JJF flotation machine to obtain scavenged concentrate and process tailings. The method is short in process, good in flotation index and low in economic cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource secondary utilization and ore dressing technology, and in particular to a column-machine combined process for recovering zinc metal from lead-zinc flotation tailings. Background Art

[0002] Most flotation tailings produced by most domestic and foreign concentrators are stored in tailings ponds. These tailings not only cause major environmental problems, but also are often rich in valuable elements such as lead, zinc, silver, sulfur, and iron due to the special properties of the ore and defects in the beneficiation process. Especially zinc, which is easy to mud and has a close relationship with sulfur embedding, has a high content in the tailings. The flotation tailings of a lead-zinc concentrator in Gansu contain a zinc grade of 0.25%~0.4%, with an annual tailings production of 1.4 million tons. The amount of zinc metal lost in the tailings is about 5,000 tons per year, which has a high recycling value. If the zinc in the tailings can be recovered, it will not only effectively improve the economic benefits of the enterprise, but also have a great reference and promotion significance for the comprehensive utilization of tailings resources of similar mines at home and abroad.

[0003] The existing lead-zinc ore production in the concentrator adopts lead-zinc priority flotation process. The flotation equipment uses JJF flotation machines of the same model but different specifications. The laboratory took an appropriate amount of representative ore samples of the tailings for zinc flotation test. After two roughing selections, one scavenging selection and three concentrating selections, the zinc concentrate grade is 31%, and the zinc recovery rate is 45%. The process has many concentrating times and the zinc recovery rate is low. In order to further explore the possibility of improving the utilization rate of zinc resources in the tailings, the particle size analysis of the tailings was carried out. The results showed that the main loss of zinc metal was in the +0.074mm and -0.038mm particle sizes. This two-level differentiated metal loss is a common mineral processing problem, because the loss of coarse-grained minerals is usually due to the failure of zinc minerals to dissociate monomers, and the grinding fineness needs to be increased to enhance recovery. Although regrinding is beneficial to the dissociation and recovery of coarse-grained minerals, it will aggravate the over-grinding of fine-grained minerals. However, the flotation machine has poor selectivity for fine-grained minerals, and this is a tailings resource with a low feed grade. In order to obtain a higher-grade zinc concentrate, the number of concentrations needs to be increased. The increase in the number of concentrations will increase the loss of fine-grained minerals, and it is difficult to take into account both the grade and recovery rate of zinc in the zinc concentrate.

[0004] The selection of flotation equipment plays a vital role in the effect of flotation technology. Flotation equipment is divided into two categories: flotation machines and flotation columns. When selecting coarse-grained minerals, the flotation machine suspends the minerals by increasing the stirring intensity of the impeller, and has a strong collection capacity, but has poor selectivity for fine-grained minerals. Compared with the flotation machine, the flotation column has a stable slurry and less agitation, which is suitable for the flotation of fine-grained minerals and has the advantage of a high concentrate enrichment ratio, but has a weak collection capacity for coarse-grained minerals.

[0005] There are many types of flotation columns, and the differences are mainly reflected in the column height, mineralization mode, bubbling mode, number of tanks, bubble generator position, etc. For example, according to the mineralization mode, it can be divided into countercurrent-collision mineralization type, cyclone-collision mineralization type, pipe flow or centrifugal-collision mineralization and various mineralization combinations; according to the bubbling mode, it can be divided into air segmentation type, air jet type, gas-liquid mixing type, etc. Over the years, improvements and innovations have been made based on the advantages and disadvantages of different column shapes, bubble generators, bubbling modes, and mineralization modes of flotation columns, and many excellent flotation columns have emerged, such as Jameson flotation column, FCSMC cyclone-static microbubble flotation column, CPT flotation column, CCF flotation column, etc. In actual application, it can be selected according to the properties of the ore to be processed and the advantages of various flotation columns. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a column-machine combined process for recovering zinc metal from lead-zinc flotation tailings, which has a short process, good flotation index and low economic cost.

[0007] In order to solve the above problems, the column-machine combined process for zinc metal recovery from lead-zinc flotation tailings described in the present invention comprises the following steps: ⑴ Stir and slurry the lead-zinc flotation tailings with zinc metal recovery value to a feed product with a concentration of 28%~30%; (2) using a CPT flotation column to perform primary zinc roughing on the feed product to obtain a primary roughing concentrate and a primary roughing tailings; (3) Classifying the primary roughing tailings to obtain a -0.074 mm fine-grained product and a +0.074 mm coarse-grained product; the fine-grained product is returned to the primary roughing operation in step (2); (4) using a JJF flotation machine to perform secondary roughing on the coarse-grained product to obtain secondary roughing concentrate and secondary roughing tailings; (5) regrinding the secondary roughing concentrate, controlling the grinding fineness to 80%-0.038 mm, and obtaining regrinding slurry; (6) The primary rougher concentrate and the reground slurry are combined and then concentrated by a CPT flotation column to obtain zinc concentrate and concentrated middlings; the concentrated middlings are returned to step (3) for classification; ⑺Use a JJF flotation machine to scavenge the secondary roughing tailings to obtain scavenge concentrate and process tailings; the scavenge concentrate is returned to step ⑷.

[0008] The zinc grade of the lead-zinc flotation tailings in step (1) is 0.2% to 0.5%.

[0009] Compared with the prior art, the present invention has the following advantages: 1. Aiming at the two-level differentiation characteristics of the loss of zinc metal in mine flotation tailings due to the distribution relationship, the present invention utilizes the respective advantages and disadvantages of flotation columns and flotation machines, and proposes to use flotation columns and flotation machines to pre-enrich fine-grained and coarse-grained zinc minerals respectively. At the same time, according to the characteristics of short flotation column flow and fast flotation speed, the fine-grained rougher concentrate and the coarse-grained flotation concentrate regrind pulp are combined, and the zinc concentrate is obtained by one-time selection by flotation columns.

[0010] 2. The CPT flotation column used in the present invention is a jet-countercurrent-microbubble flotation column. The cavity resonant foamer in the flotation column uses the jet principle to generate microbubbles. The microbubbles are small in diameter and can selectively precipitate on the surface of hydrophobic minerals. The microbubbles are mostly in a laminar state, which makes it easy for fine materials to be adsorbed and not easy to fall off. In addition, the countercurrent flotation column has a low absolute speed of movement of particles and bubbles because the particles and bubbles move in opposite directions and the turbulence degree is low. It not only provides a large number of opportunities for bubbles to capture mineral particles, but also the coarse-grained minerals attached to the bubbles are not easy to fall off. Compared with the downstream and cyclone flotation columns, the countercurrent flotation column has obvious advantages in capturing coarse-grained minerals.

[0011] 3. Compared with the conventional full flotation machine process, the process of the present invention for recovering zinc resources from tailings has the advantages of short process, low cost and good flotation index. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0013] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0014] like Figure 1 As shown, a column-machine combined process for zinc metal recovery from lead-zinc flotation tailings comprises the following steps: ⑴ Stir and slurry the lead-zinc flotation tailings with zinc metal recovery value and zinc grade of 0.2%~0.5% to adjust the concentration to 28%~30% of the feed product; (2) Use CPT flotation column (produced by Canadian CPT company) to carry out primary roughing of zinc on the feed product to obtain primary roughing concentrate and primary roughing tailings; (3) Classify the primary roughing tailings to obtain -0.074mm fine-grained products and +0.074mm coarse-grained products; the fine-grained products are returned to the primary roughing operation in step (2); (4) Use JJF flotation machine to conduct secondary roughing of coarse-grained products to obtain secondary roughing concentrate and secondary roughing tailings; (5) Regrind the secondary roughing concentrate, control the grinding fineness to 80%-0.038mm, and obtain the regrinding slurry; (6) The primary rougher concentrate and the reground slurry are combined and then concentrated by CPT flotation column to obtain zinc concentrate and concentrated middlings; the concentrated middlings are returned to step (3) for classification; ⑺Use JJF flotation machine to scavenge the secondary roughing tailings to obtain scavenge concentrate and process tailings; the scavenge concentrate is returned to step ⑷.

[0015] Working principle: In view of the low zinc grade (0.2%~0.5%) in flotation tailings and the two-level differentiation of zinc metal particle size, combined with the respective advantages of flotation machines and flotation column equipment, especially the jet-countercurrent-microbubble CPT flotation column has good collection performance for coarse and fine-grained minerals, the CPT flotation column is first used to pre-roughly enrich part of the fine-grained zinc metal, the tailings of the first roughing are classified, the fine-grained classified products are returned to the roughing, and the coarse-grained products are subjected to secondary roughing and scavenging by the JJF flotation machine. Then, by taking advantage of the short process and fast flotation speed of the CPT flotation column, the enriched fine-grained rough concentrate and the re-grinded coarse-grained rough concentrate are combined and then subjected to a first concentration by the CPT flotation column to obtain the zinc concentrate. At the same time, the concentrated middlings are returned to the classification operation, and the scavenged concentrate is returned to the secondary roughing process.

[0016] Example 1 A lead-zinc flotation tailings, zinc grade 0.35%, using Figure 1 The process flow shown in the figure is used to recover the tailings. The specific reagent conditions are as follows: 1000g / t lime, 150g / t copper sulfate, 40g / t butyl xanthate are added in the first roughing process. # Oil 20g / t, secondary roughing add butyl xanthate 15g / t, 2 # Oil 5g / t, butyl xanthate 5g / t is added for scavenging, and lime 500g / t is added for concentrating.

[0017] The conventional scheme is to use the same reagent conditions as above, and flotation machines are used for roughing, scavenging and concentrating. Zinc concentrate is obtained after two roughing, one scavenging and three concentrating.

[0018] The comparison of the test indicators obtained by using the above two process schemes is shown in Table 1.

[0019] Table 1 Comparison of test results of Example 1 It can be seen from Table 1 that the zinc concentrate obtained by the process of the present invention is superior to the conventional process in terms of grade and recovery rate, and the process structure is short and easier to implement.

[0020] Example 2 A copper-zinc flotation tailings, zinc grade 0.25%, using Figure 1The process flow shown in the figure is used to recover the tailings. The specific reagent conditions are as follows: 1000g / t lime, 100g / t copper sulfate, 30g / t butyl xanthate are added in the first roughing process. # Oil 15g / t, secondary roughing add butyl xanthate 10g / t, 2 # Oil 5g / t, butyl xanthate 5g / t is added for scavenging, and lime 500g / t is added for concentrating.

[0021] The conventional scheme is to use the same reagent conditions as above, and flotation machines are used for roughing, scavenging and concentrating. Zinc concentrate is obtained after two roughing, one scavenging and three concentrating.

[0022] The comparison of the test indicators obtained by using the above two process schemes is shown in Table 2.

[0023] Table 2 Comparison of test results of Example 2 It can be seen from Table 2 that, compared with the conventional process scheme, the process of the present invention not only has a short process structure and is easy to implement, but also has good zinc flotation indicators.

[0024] Example 3 A copper-lead-zinc polymetallic flotation tailings, zinc grade 0.5%, using Figure 1 The process flow shown in the figure is used to recover the tailings. The specific reagent conditions are as follows: 1000g / t lime, 200g / t copper sulfate, 50g / t butyl xanthate are added in the first roughing process. # Oil 20g / t, secondary roughing add butyl xanthate 15g / t, 2 # Oil 5g / t, butyl xanthate 5g / t is added for scavenging, and lime 500g / t is added for concentrating.

[0025] The conventional scheme is to use the same reagent conditions as above, and flotation machines are used for roughing, scavenging and concentrating. Zinc concentrate is obtained after two roughing, one scavenging and three concentrating.

[0026] The comparison of the test indicators obtained by using the above two process schemes is shown in Table 3.

[0027] Table 3 Comparison of test results of Example 3 It can be seen from Table 3 that, compared with the conventional process scheme, the process of the present invention not only has a short process structure and is easy to implement, but also has good zinc flotation indicators.

Claims

1. A column-machine combined process for recovering zinc metal from lead-zinc flotation tailings, comprising the following steps: ⑴ Stir and slurry the lead-zinc flotation tailings with zinc metal recovery value to a feed product with a concentration of 28%~30%; (2) using a CPT flotation column to perform primary zinc roughing on the feed product to obtain a primary roughing concentrate and a primary roughing tailings; (3) Classifying the primary roughing tailings to obtain a -0.074 mm fine-grained product and a +0.074 mm coarse-grained product; the fine-grained product is returned to the primary roughing operation in step (2); (4) using a JJF flotation machine to perform secondary roughing on the coarse-grained product to obtain secondary roughing concentrate and secondary roughing tailings; (5) regrinding the secondary roughing concentrate, controlling the grinding fineness to 80%-0.038 mm, and obtaining regrinding slurry; (6) The primary rougher concentrate and the reground slurry are combined and then concentrated by a CPT flotation column to obtain zinc concentrate and concentrated middlings; the concentrated middlings are returned to step (3) for classification; ⑺Use a JJF flotation machine to scavenge the secondary roughing tailings to obtain scavenge concentrate and process tailings; the scavenge concentrate is returned to step ⑷.

2. A column-machine combined process for zinc metal recovery from lead-zinc flotation tailings as claimed in claim 1, characterized in that: The zinc grade of the lead-zinc flotation tailings in step (1) is 0.2% to 0.5%.

Citation Information

Patent Citations

  • Method for sorting and separating ore from aluminum silicon mineral

    CN101176863A

  • Technology for flotation of lead and zinc sulfide ores through inflatable floatation columns

    CN103934117A

  • Machine-column-machine rapid and efficient zinc flotation method and system

    CN109647614A

  • Beneficiation method and beneficiation system for efficiently improving recycling rate of difficult-to-separate zinc concentrate

    CN109647615A

  • Method for improving recovery rate of gold in semi-primary semi-oxidized gold ore by full flotation process