Method for improving ore grinding efficiency and grade of iron ore concentrate
By adopting semi-self-grinding and multi-stage magnetic separation processes in vanadium titanium magnetite ore dressing, combining tower grinding and grading, the problems of long process flow, low grinding efficiency and high dust are solved, and efficient iron concentrate production is achieved. Significantly improves iron concentrate grade and grinding efficiency.
Patent Information
- Application Number
- CN202411284994.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-05
AI Technical Summary
The existing vanadium titanium magnetite production process is long, the grinding efficiency is low, the dust is generated, and the iron concentrate grade is low.
The semi-self-grinding process is used to replace the traditional three-stage, one closed-circuit crushing and one-stage ball milling process. Through multi-stage magnetic separation and tower milling process, combining grading and dehydration magnetic separation, dispersant assisted tower milling is used to shorten the iron selection process, improve grinding efficiency and grade.
The iron concentrate classification process has been significantly shortened, the grinding efficiency and grade have been improved, dust emissions have been reduced, ball milling and grading efficiency have been improved, and high-grade iron concentrate has been obtained.
Smart Images

Figure CN118892912A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a method for improving the grinding efficiency and grade of iron ore concentrate. Background Art
[0002] At present, the mainstream process adopted for the beneficiation of vanadium-titanium magnetite is: three-stage one closed-circuit crushing → one-stage ball mill grinding → cyclone classification → one-stage magnetic separation → two-stage ball milling → two-stage cyclone classification → two-stage high-frequency screen classification → two-stage magnetic separation. The main disadvantages of this process are that the process is relatively long, and there are many positions due to the large number of equipment. At the same time, both stages of grinding use ball mills as grinding equipment, which has low grinding efficiency, coarse grinding particle size, and it is difficult to improve the grade of concentrate. Secondly, the three-stage one closed-circuit crushing process has large dust and poor working environment.
[0003] CN101480632B discloses a beneficiation method for pure magnetite, wherein the raw ore is sequentially crushed, first-stage dry magnetic separation, medium crushing, second-stage dry magnetic separation, fine crushing, and third-stage dry magnetic separation, and a large amount of gangue is thrown out through the third-stage dry magnetic separation to obtain powder ore, which is sent to the grinding head screen for screening, and the fine particles screened by the grinding head screen enter the first magnetic separation process, and the coarse materials screened by the grinding head screen are subjected to a first ball milling, and then enter the first magnetic separation process, and the ore materials after the first magnetic separation are discharged from the tailings sand, and then enter the second ball milling to ensure that the particle size of the mineral fine powder is -200 mesh ≥ 60%, and the fine powder after the second ball milling enters the second magnetic separation, and the ore materials after the second magnetic separation are discharged from the tailings sand and enter the high-frequency screen, and the product on the screen is filtered to obtain the concentrate; the product under the screen is desludged and then floated. The beneficiation process of this method is a complete three-stage one closed-circuit crushing + two-stage grinding and selection process, and the process flow is complicated and the efficiency is low.
[0004] CN117983397A discloses a method for selecting high-quality iron concentrate from ultra-low-grade vanadium-titanium magnetite, and relates to the field of mineral processing technology. The method includes the following process flows: a three-stage fully closed-circuit grinding and grading process flow, a "screening before grinding" process flow, a "step grinding and step selection" process flow, a "high-frequency stacked screen + cyclone" combined grading and a cyclone grading process, etc. Through the combined application of the above processes, the problems of low quality, high cost and high operation difficulty of selecting iron concentrate from ultra-low-grade vanadium-titanium magnetite can be effectively solved, the grade and fineness of the iron concentrate can be improved, the production cost can be reduced, and the production efficiency can be improved. In the ore dressing process of the method, there are many grinding steps, a long process flow, and a very low grinding efficiency; the iron grade in the obtained iron concentrate is >54%, and the iron concentrate grade is low.
[0005] In view of this, it is necessary to develop a new vanadium-titanium magnetite beneficiation method. Summary of the invention
[0006] The technical problem to be solved by the present invention is that the existing process of producing iron concentrate from vanadium-titanium magnetite is long, the grinding efficiency is low, the dust is high and the grade of the iron concentrate is low.
[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for improving the grinding efficiency and grade of iron ore concentrate, comprising the following steps:
[0008] a. The raw ore is screened after semi-autogenous grinding;
[0009] a1. The screen returns to the semi-autogenous grinding mill for re-grinding;
[0010] a2. The sieve enters a magnetic separation stage for tailings disposal to obtain magnetic concentrate 1 and magnetic tailings 1;
[0011] b. The magnetic concentrate 1 enters the second stage ball mill, and the ball mill discharge undergoes the second stage magnetic separation to obtain the magnetic concentrate 2 and the magnetic tailings 2;
[0012] c. The magnetic concentrate 2 is passed through a high-frequency fine screen for classification;
[0013] c1. Dehydration and magnetic separation are performed on the sieve to obtain dehydrated magnetic concentrate and dehydrated magnetic tailings. The dehydrated magnetic concentrate is returned to step b and mixed with the magnetic concentrate 1 to enter the second stage ball mill. The dehydrated magnetic tailings are returned to step b and mixed with the ball mill discharge for second stage magnetic separation;
[0014] c2. The screen enters the three-stage magnetic separation to obtain magnetic concentrate 3 and magnetic tailings 3;
[0015] d. The magnetic concentrate 3 is subjected to three-stage tower milling, a dispersant is added to the tower mill, and a cyclone is used for classification after the tower milling to obtain classified sand and classified overflow, and the classified sand is returned to step d and mixed with the magnetic concentrate 3 for three-stage tower milling;
[0016] e. The classified overflow is subjected to four-stage magnetic separation to obtain iron concentrate with a TFe grade of 61.0% to 63.5% and tailings with a TFe grade of 10% to 11.5%.
[0017] In the above step a, the screening particle size is 1 mm to 5 mm.
[0018] Furthermore, in step a2, the magnetic separation intensity of one stage of magnetic separation is 2000 Gs to 4000 Gs.
[0019] In the above step b, the concentration of the second stage ball milling is 65% to 78%; the magnetic separation intensity of the second stage magnetic separation is 2000 Gs to 3000 Gs.
[0020] In the above step c, the classification particle size is 0.038 mm to 0.25 mm.
[0021] Furthermore, in step c1, the magnetic separation intensity of the dehydration magnetic separation is 2000 Gs to 4000 Gs.
[0022] Furthermore, in step c2, the magnetic separation intensity of the three-stage magnetic separation is 1000Gs to 2000Gs.
[0023] In the above step d, the amount of dispersant added is 10-400 g / t, and the components of the dispersant are 70%-90% soda and 10%-30% water glass in mass percentage; the discharge particle size of the three-stage tower mill is -400 mesh, accounting for 70%-99%; and a 400-mesh cyclone is used for classification.
[0024] In the above step e, the magnetic separation intensity of the four-stage magnetic separation is 2000Gs to 3000Gs.
[0025] In the above method for improving the grinding efficiency and grade of iron ore concentrate, the magnetic separation tailings 1 are used as raw materials for coarse particle removal and titanium recovery; the magnetic separation tailings 2 and the magnetic separation tailings 3 are used as raw materials for fine particle titanium recovery.
[0026] The beneficial effects of the present invention are as follows: the present invention provides a method for improving the grinding efficiency and grade of iron ore concentrate, adopts a semi-autogenous grinding process to replace the three-stage one-closed-circuit crushing and one-stage ball milling process in the traditional process, shortens the iron selection process, and at the same time, due to wet grinding, there is no dust, thereby reducing dust emission; the first tailings are discarded through a first-stage magnetic separation, thereby reducing the amount of ball mill input, and improving the ball milling efficiency and energy consumption; the second tailings are discarded through a second-stage magnetic separation, thereby reducing the amount of ore entering the grading system, improving the grading efficiency, and accelerating the iron selection process; the concentration of the ore entering the ball mill is increased through a three-stage magnetic separation; a dispersant is used to assist the tower mill to improve the grinding effect, and a high-grade iron ore concentrate is obtained through subsequent grading and magnetic separation.
[0027] The method for improving the grinding efficiency and grade of iron ore concentrate of the present invention significantly shortens the iron ore separation process, improves the grinding efficiency of iron ore concentrate, effectively improves the grade of iron ore concentrate, and has a high prospect for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0029] The technical scheme of the present invention can be specifically implemented in the following manner. Those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0030] Embodiment 10,000 tons of vanadium-titanium magnetite with a TFe grade of 28.2% were collected, and iron concentrate was produced according to the method of improving the grinding efficiency and grade of iron concentrate of the present invention. The specific process is as follows:
[0031] The raw ore is screened after semi-autogenous grinding, and the screening particle size is 2.5mm. The ore on the screen is returned to the semi-autogenous mill for re-grinding, and the ore under the screen enters the first magnetic separation (magnetic separation intensity 3000Gs) for tailings to obtain magnetic separation concentrate 1; the magnetic separation concentrate 1 enters the second ball mill (concentration 70%), and the ball mill discharge is subjected to the second magnetic separation (magnetic separation intensity 2500Gs) to obtain magnetic separation concentrate 2; the magnetic separation concentrate 2 is passed through a high-frequency fine screen for classification, and the classification particle size is 0.1mm. Dehydration magnetic separation (magnetic field intensity 3000Gs) is performed on the screen to obtain dehydrated magnetic separation concentrate and dehydrated magnetic separation tailings, and the dehydrated magnetic separation concentrate returns to step b and is mixed with the magnetic separation concentrate 1 After entering the second stage ball mill, the dehydrated magnetic tailings are returned to step b and mixed with the ball mill discharge for the second stage magnetic separation; the screen enters the third stage magnetic separation (magnetic separation intensity 1500Gs) to obtain magnetic concentrate 3; the magnetic concentrate 3 is subjected to the third stage tower mill, and a dispersant (a mixture of 80% soda and 20% water glass) is added to the tower mill at an amount of 200g / t. After the tower mill, a cyclone classification (400 mesh) is performed to obtain graded sand and graded overflow, and the graded sand is returned to step d and mixed with the magnetic concentrate 3 for the third stage tower mill; the graded overflow is subjected to the fourth stage magnetic separation (magnetic separation intensity 3000Gs) to obtain iron concentrate and tailings.
[0032] In the embodiment, the output of the second stage grinding new-200 mesh is 1.35t / (h·m 3 ), the particle size of the tower mill discharge is -400 mesh 93.12%, and the iron ore TFe grade is 63.21%.
[0033] In the comparative example, 10,000 tons of vanadium-titanium magnetite with a TFe grade of 28.2% as in the example was used to produce iron concentrate according to the conventional process. The process parameters were set the same as in the example. The specific process was as follows:
[0034] The raw ore is crushed in three stages in one closed circuit → ground in one stage ball mill → classified in cyclone → classified in one stage magnetic separation → second stage ball mill → second stage cyclone classification → second stage high frequency screen classification → second stage magnetic separation process. The second stage magnetic separation concentrate is ground in tower mill and then classified to obtain cyclone overflow and cyclone sand settling. The cyclone overflow enters the three-stage magnetic separation to obtain iron concentrate and tailings.
[0035] The output of the second-stage grinding of the comparative example is 0.98t / (h·m 3 ), the tower mill discharge particle size is -400 mesh 86.34%, and the iron concentrate TFe grade is 56.34%. It can be seen that the method for improving the grinding efficiency and grade of iron concentrate of the present invention is used to produce iron concentrate, which significantly improves the grinding efficiency, reduces the grinding particle size, and improves the concentrate grade compared with the traditional process for producing iron concentrate.
Claims
1. A method for improving the grinding efficiency and grade of iron ore concentrate, characterized in that: The steps include: a. The raw ore is screened after semi-autogenous grinding; a1. The screen returns to the semi-autogenous grinding mill for re-grinding; a2. The sieve enters a magnetic separation stage for tailings disposal to obtain magnetic concentrate 1 and magnetic tailings 1; b. The magnetic concentrate 1 enters the second stage ball mill, and the ball mill discharge undergoes the second stage magnetic separation to obtain the magnetic concentrate 2 and the magnetic tailings 2; c. The magnetic concentrate 2 is passed through a high-frequency fine screen for classification; c1. Dehydration and magnetic separation are performed on the sieve to obtain dehydrated magnetic concentrate and dehydrated magnetic tailings. The dehydrated magnetic concentrate is returned to step b and mixed with the magnetic concentrate 1 to enter the second stage ball mill. The dehydrated magnetic tailings are returned to step b and mixed with the ball mill discharge for second stage magnetic separation; c2. The screen enters the three-stage magnetic separation to obtain magnetic concentrate 3 and magnetic tailings 3; d. The magnetic concentrate 3 is subjected to three-stage tower milling, a dispersant is added to the tower mill, and a cyclone is used for classification after the tower milling to obtain classified sand and classified overflow, and the classified sand is returned to step d and mixed with the magnetic concentrate 3 for three-stage tower milling; e. The classified overflow is subjected to four-stage magnetic separation to obtain iron concentrate with a TFe grade of 61.0% to 63.5% and tailings with a TFe grade of 10% to 11.5%.
2. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step a, the screening particle size is 1 mm to 5 mm.
3. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step a2, the magnetic separation intensity of the first stage of magnetic separation is 2000 Gs to 4000 Gs.
4. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step b, the concentration of the second stage ball milling is 65% to 78%; the magnetic separation intensity of the second stage magnetic separation is 2000 Gs to 3000 Gs.
5. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step c, the classification particle size is 0.038 mm to 0.25 mm.
6. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step c1, the magnetic separation intensity of the dehydration magnetic separation is 2000Gs to 4000Gs.
7. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step c2, the magnetic separation intensity of the three-stage magnetic separation is 1000Gs to 2000Gs.
8. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step d, the amount of dispersant added is 10-400 g / t, and the components of the dispersant are 70%-90% soda and 10%-30% water glass by mass percentage; the discharge particle size of the three-stage tower mill is -400 mesh, accounting for 70%-99%; and a 400-mesh cyclone is used for classification.
9. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: In step e, the magnetic separation intensity of the four-stage magnetic separation is 2000Gs to 3000Gs.
10. The method for improving the grinding efficiency and grade of iron ore concentrate according to claim 1, characterized in that: The magnetic separation tailings 1 are used as raw materials for coarse particle titanium separation and recovery; the magnetic separation tailings 2 and magnetic separation tailings 3 are used as raw materials for fine particle titanium separation and recovery.
Citation Information
Patent Citations
Mineral separation process of magnetic iron ore
CN101480632B
Method for separating high-quality iron ore concentrate from ultralow-grade vanadium titano-magnetite
CN117983397A
Low-cost high-recovery environment-friendly mineral separation method of low-grade vanadium titano-magnetite
CN105107616A
Magnetite beneficiation method
CN110152876A
Fine-particle magnetite beneficiation process
CN111068897A
Cited By