Cerium oxide super-hydrophilic / super-hydrophobic array fog collection film and preparation method thereof

The cerium oxide nanosphere film was prepared by sol-gel method and hydrothermal synthesis method, and the ultra-hydrophilic/super-hydrophobic array was constructed using molecular self-assembly and deep ultraviolet radiation technology, which solved the low mist capture efficiency of existing mist collecting films The problem is that efficient fog capture and fog collection cycle is achieved.

CN118892982AActive Publication Date: 2024-11-05XIAN UNIV OF TECH

Patent Information

Application Number
CN202410928057.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing mist-capturing films have low mist capture efficiency, and the growth rate of droplets condensed on the surface of the superhydrophobic films is slow, which hinders subsequent droplet condensation and leads to low mist capture efficiency.

Method used

The cerium oxide nanosphere film was prepared by sol-gel method and hydrothermal synthesis method, and low surface energy modification was carried out through molecular self-assembly technology, and superhydrophilic/superhydrophobic array was constructed in combination with deep ultraviolet radiation technology to improve droplet nucleation with capture efficiency.

Benefits of technology

The nucleation and capture efficiency of fog droplets is significantly improved, and the superhydrophobic region controls the adhesion of the droplets to roll down, thereby achieving efficient fog capture and fog collection cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892982A_ABST
    Figure CN118892982A_ABST
Patent Text Reader

Abstract

The invention discloses a cerium oxide super-hydrophilic / super-hydrophobic array fog collection film and a preparation method thereof. The preparation method comprises the following specific steps: step 1, preparing a cerium oxide film on a silicon substrate by using a sol-gel method; step 2, immobilizing nanospheres on the surface of the cerium oxide film by using a hydrothermal synthesis method to obtain a cerium oxide nanosphere film; step 3, performing low surface energy modification on the cerium oxide film with the nanosphere structure on the surface by using a molecular self-assembly technology to obtain a super-hydrophobic cerium oxide nanosphere film; and 4, covering the surface of the super-hydrophobic cerium oxide nanosphere film with mask plates of different specifications, and performing deep ultraviolet radiation to obtain the cerium oxide super-hydrophilic / super-hydrophobic array fog collection film. The mist collection film can realize efficient mist capture and mist collection circulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fog collecting films, and in particular relates to a preparation method of a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film, and also relates to a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film. Background Art

[0002] Collecting water from fog is a sustainable solution to the water shortage problem in some areas. Among the existing fog collection equipment and materials, fog collection films have become a hot topic of research due to their large contact area with fog and wide applicability. Most of the existing fog collection films are super-hydrophobic films. Since the droplets condensed on the surface of super-hydrophobic films grow slowly and once they cover the surface of the substrate, they will hinder the condensation of subsequent droplets, so their fog capture efficiency is not high. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film, which solves the problem of low fog capturing efficiency of the existing fog collecting film.

[0004] Another object of the present invention is to provide a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0005] The technical solution adopted by the present invention is a method for preparing a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film, which is specifically implemented according to the following steps:

[0006] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0007] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0008] Step 3, using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0009] Step 4, covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and using deep ultraviolet irradiation to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0010] The present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Step 1.1, adding cerium (III) acetate hydrate into anhydrous methanol to dissolve, then adding catalyst propionic acid, sealing, stirring, standing and aging, to obtain cerium oxide sol;

[0013] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dipping-pulling method;

[0014] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film.

[0015] In step 1.1, the concentration of the cerium oxide sol is 0.10 mol / L to 0.80 mol / L, and the molar ratio of cerium (III) acetate hydrate to propionic acid is 1:3.

[0016] In step 1.2, the pulling speed of the immersion-pulling method is 0.5 mm / s to 4 mm / s;

[0017] In step 1.3, the heat treatment process is: first keep warm at 200°C for 10 minutes, then heat from 200°C to 800°C and keep warm for 15 minutes, repeat the above treatment process 3 times, and keep warm at 800°C for 2 hours for the third time.

[0018] The specific process of step 2 is:

[0019] Step 2.1, using cerium nitrate hexahydrate as a cerium source and urea as an alkali source, fully dissolving them in deionized water, and after the solution is completely clarified, obtaining a cerium oxide hydrothermal reaction solution;

[0020] Step 2.2, placing the cerium oxide film obtained in step 1 in a polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pouring the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner, placing the polytetrafluoroethylene liner in a hydrothermal kettle for reaction, cooling to room temperature with the furnace, and taking out the sample after the reaction is completed;

[0021] Step 2.3, using deionized water and anhydrous ethanol to alternately wash the excess cerium oxide nanopowder attached to the surface of the sample, and drying and annealing the washed sample to obtain a cerium oxide nanosphere film.

[0022] In step 2.1, the concentration of the cerium oxide hydrothermal reaction solution is 0.010 mol / L to 0.080 mol / L;

[0023] In step 2.2, the reaction temperature in the hydrothermal reactor is 100°C and the reaction time is 24h;

[0024] In step 2.3, the drying temperature is 60°C to 80°C, and the drying time is 10min to 20min; the annealing process is: raising the temperature to 450°C in a muffle furnace at a heating rate of 3°C / min to 5°C / min and keeping it warm for 2h.

[0025] The specific process of step 3 is: immersing the cerium oxide nanosphere film obtained in step 2 in a low surface energy modifier solution for modification, taking it out and washing it with anhydrous ethanol to remove the modifier remaining on the surface, and drying it to obtain a super hydrophobic cerium oxide nanosphere film.

[0026] The concentration of the low surface energy modifier solution is 15g / L to 60g / L, the low surface energy modifier is one of octadecyltrimethyloxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, hexadecyltrimethyloxysilane, and vinyltrimethoxysilane, the solvent is anhydrous ethanol, the immersion modification time is 10min to 50min, the drying temperature is 25℃ to 80℃, and the time is 10min to 30min.

[0027] The specific process of step 4 is: covering the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3 with a mask having a specific pattern, and then irradiating the unmasked area with deep ultraviolet light at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0028] The wavelength of ultraviolet light is 180nm~280nm, and the irradiation time is 3h~8h.

[0029] Another technical solution adopted by the present invention is that the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film is obtained by adopting the above-mentioned preparation method.

[0030] The beneficial effects of the present invention are as follows: the preparation method of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film of the present invention first adopts a sol-gel method combined with a hydrothermal synthesis method to prepare a surface-dense cerium oxide nanosphere film, then uses molecular self-assembly technology to perform low surface energy modification on it, and then uses deep ultraviolet radiation-assisted mask technology to construct an array with super-hydrophilic and super-hydrophobic regions alternating regularly, wherein the super-hydrophilic region of the film significantly improves the efficiency of droplet nucleation and capture, and the super-hydrophobic region controls the size of droplets adhered to the fog collecting surface, so that they can roll off the fog collecting surface when they grow to a certain extent, allowing the super-hydrophilic region to re-contact and capture the droplets, thereby achieving efficient fog capture and fog collection cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the XRD diagram of the cerium oxide film prepared by the method of the present invention before and after hydrothermal treatment;

[0032] Figure 2 This is a contact angle picture of the super-hydrophobic cerium oxide nanosphere film prepared by the method of the present invention;

[0033] Figure 3 This is a picture of the rolling angle of the super-hydrophobic cerium oxide nanosphere film prepared by the method of the present invention;

[0034] Figure 4This is a SEM image of a cerium oxide super-hydrophilic / super-hydrophobic array fog-collecting film prepared by the method of the present invention;

[0035] Figure 5 This is an EDS electron layered image of a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention;

[0036] Figure 6 This is the EDS spectrum of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention;

[0037] Figure 7 It is a Ce element distribution diagram of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention;

[0038] Figure 8 It is the distribution diagram of O element of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention;

[0039] Fig. 9 It is the F element distribution diagram of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention;

[0040] Fig.10 It is a C element distribution diagram of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention. DETAILED DESCRIPTION

[0041] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0042] The preparation method of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film of the present invention is specifically implemented according to the following steps:

[0043] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0044] The specific process is:

[0045] Step 1.1, adding cerium (III) acetate hydrate to anhydrous methanol to dissolve, then adding catalyst propionic acid, sealing, stirring for 2h to 10h, and standing for aging for 24h to obtain cerium oxide sol;

[0046] The concentration of the cerium oxide sol is 0.10 mol / L to 0.80 mol / L, and the molar ratio of cerium (III) acetate hydrate to propionic acid is 1:3;

[0047] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dipping-pulling method;

[0048] Among them, the pulling speed is 0.5mm / s~4mm / s;

[0049] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0050] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above treatment process 3 times, and keep the temperature at 800°C for 2 hours for the third time;

[0051] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0052] The specific process is:

[0053] Step 2.1, using cerium nitrate hexahydrate as a cerium source and urea as an alkali source, fully dissolving them in deionized water, and after the solution is completely clarified, obtaining a cerium oxide hydrothermal reaction solution;

[0054] Wherein, the concentration of the cerium oxide hydrothermal reaction solution is 0.010 mol / L to 0.080 mol / L;

[0055] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0056] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0057] The drying temperature is 60°C to 80°C, and the drying time is 10min to 20min. The annealing process is: the temperature is raised to 450°C in a muffle furnace at a heating rate of 3°C / min to 5°C / min and kept at this temperature for 2h.

[0058] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0059] The specific process is:

[0060] The cerium oxide nanosphere film obtained in step 2 is placed in a low surface energy modifier solution for 10 to 50 minutes, taken out and washed with anhydrous ethanol to remove the modifier remaining on the surface, and dried to obtain a super-hydrophobic cerium oxide nanosphere film;

[0061] The concentration of the low surface energy modifier solution is 15 g / L to 60 g / L, the low surface energy modifier is one of octadecyl trimethyloxysilane, 1H, 1H, 2H, 2H-perfluorodecyl trimethoxysilane, hexadecyl trimethyloxysilane, and vinyl trimethoxysilane, and the solvent is anhydrous ethanol.

[0062] The drying temperature is 25℃~80℃ and the drying time is 10min~30min;

[0063] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0064] The specific process is:

[0065] Covering the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3 with a mask having a specific pattern, and then irradiating the unmasked area with deep ultraviolet light at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0066] Among them, the wavelength of ultraviolet light is 180nm~280nm, and the irradiation time is 3h~8h.

[0067] The super-hydrophilic region in the cerium oxide super-hydrophilic / super-hydrophobic array fog-collecting film obtained by the present invention has a large adhesion force to the fog droplets, can quickly capture the fog droplets in the air, and make them aggregate with each other to form larger droplets; the super-hydrophobic region has a low surface free energy and a high contact angle, and has extremely weak adhesion force to the fog droplets, so that the fog droplets can quickly roll off the surface of the sample; the super-hydrophilic and super-hydrophobic regions are regularly and alternately arranged, which can not only accelerate the convergence growth of the fog droplets and significantly improve the nucleation and capture efficiency of the fog droplets, but also when the fog droplets reach a critical size, they can quickly roll off the surface of the array fog-collecting film under the action of the low adhesion force of the super-hydrophobic region or gravity, so that the super-hydrophilic region can re-contact and capture the fog droplets, and repeat over and over again, thereby realizing an efficient fog capture and fog collection cycle.

[0068] Example 1

[0069] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0070] The specific process is:

[0071] Step 1.1, 0.6345 g of cerium (III) acetate hydrate was added to 20 mL of anhydrous methanol and dissolved, and then 0.4445 g of catalyst propionic acid was added, the mixture was sealed and stirred at room temperature for 3 h on a magnetic stirrer, and then aged for 24 h to obtain a yellow-brown transparent cerium oxide sol with a concentration of 0.10 mol / L;

[0072] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dip-pulling method at a pulling speed of 0.5 mm / s;

[0073] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0074] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above process 3 times, and keep the temperature at 800°C for 2 hours for the third time; during this heat treatment process, the polymer will gradually decompose to form cerium oxide, and the cerium oxide film will be obtained as the substrate of the hydrothermal method;

[0075] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0076] The specific process is:

[0077] Step 2.1, 0.1303 g of cerium nitrate hexahydrate as a cerium source and 0.0540 g of urea as an alkali source are fully dissolved in 30 mL of deionized water, and after the solution is completely clarified, a hydrothermal reaction solution of cerium oxide with a concentration of 0.010 mol / L is obtained;

[0078] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0079] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0080] The drying temperature is 80°C and the drying time is 10 to 20 minutes. The annealing process is as follows: the temperature is raised to 450°C at a heating rate of 3°C / min in a muffle furnace and kept at this temperature for 2 hours.

[0081] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0082] The specific process is:

[0083] The cerium oxide nanosphere film obtained in step 2 is immersed in an anhydrous ethanol solution of octadecyltrimethyloxysilane with a concentration of 15 g / L for modification for 15 min, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and then dried at 80° C. for 10 min to 30 min, and then a layer of perfluorosilane is self-assembled on the surface of the cerium oxide to obtain a super-hydrophobic cerium oxide nanosphere film;

[0084] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0085] The specific process is:

[0086] A mask with a stripe size of 1 mm × 5 cm was covered on the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 280 nm was irradiated on the unmasked area for 3 h at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0087] like Figure 1 As shown, a is the curve before hydrothermal treatment and b is the curve after hydrothermal treatment. It can be seen that the diffraction intensity of the cerium oxide film is significantly improved after hydrothermal treatment.

[0088] Example 2

[0089] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0090] The specific process is:

[0091] Step 1.1, 0.95 g of cerium (III) acetate hydrate was dissolved in 20 mL of anhydrous methanol, and then 0.67 g of catalyst propionic acid was added, the mixture was sealed, stirred at room temperature for 4 h on a magnetic stirrer, and aged for 24 h to obtain a yellow-brown transparent cerium oxide sol with a concentration of 0.30 mol / L;

[0092] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dip-pulling method at a pulling speed of 1.5 mm / s;

[0093] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0094] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above process 3 times, and keep the temperature at 800°C for 2 hours for the third time; during this heat treatment process, the polymer will gradually decompose to form cerium oxide, and the cerium oxide film will be obtained as the substrate of the hydrothermal method;

[0095] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0096] The specific process is:

[0097] Step 2.1, 0.3908 g of cerium nitrate hexahydrate as a cerium source and 0.2700 g of urea as an alkali source are fully dissolved in 30 mL of deionized water, and after the solution is completely clarified, a hydrothermal reaction solution of cerium oxide with a concentration of 0.030 mol / L is obtained;

[0098] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0099] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0100] The drying temperature is 80°C and the drying time is 10-20 minutes. The annealing process is as follows: the temperature is raised to 450°C at a heating rate of 5°C / min in a muffle furnace and kept at this temperature for 2 hours.

[0101] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0102] The specific process is:

[0103] The cerium oxide nanosphere film obtained in step 2 is immersed in an anhydrous ethanol solution of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane with a concentration of 50 g / L for 10 min, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and then dried at 80° C. for 10 min to 30 min, and then a layer of perfluorosilane is self-assembled on the surface of the cerium oxide to obtain a super-hydrophobic cerium oxide nanosphere film;

[0104] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0105] The specific process is:

[0106] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 280 nm is irradiated on the unmasked area for 4 hours at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0107] like Figure 2 and Figure 3 As shown, the contact angle is 167.2° and the sliding angle is 1.8° , This indicates that the surface of the cerium oxide nanosphere film prepared at this concentration has extremely low adhesion and excellent surface hydrophobicity, and the captured small droplets can roll off quickly when in contact with the sample surface.

[0108] Example 3

[0109] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0110] The specific process is:

[0111] Step 1.1, 3.1725 g of cerium (III) acetate hydrate was added to 20 mL of anhydrous methanol and dissolved, and then 2.2224 g of catalyst propionic acid was added, the mixture was sealed and stirred at room temperature for 6 h on a magnetic stirrer, and then aged for 24 h to obtain a yellow-brown transparent cerium oxide sol with a concentration of 0.50 mol / L;

[0112] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dip-pulling method at a pulling speed of 2 mm / s;

[0113] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0114] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above process 3 times, and keep the temperature at 800°C for 2 hours for the third time; during this heat treatment process, the polymer will gradually decompose to form cerium oxide, and the cerium oxide film will be obtained as the substrate of the hydrothermal method;

[0115] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0116] The specific process is:

[0117] Step 2.1, 0.6513 g of cerium nitrate hexahydrate as a cerium source and 0.2703 g of urea as an alkali source are fully dissolved in 30 mL of deionized water, and after the solution is completely clarified, a hydrothermal reaction solution of cerium oxide with a concentration of 0.050 mol / L is obtained;

[0118] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0119] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0120] The drying temperature is 80°C and the drying time is 10-20 minutes. The annealing process is as follows: the temperature is raised to 450°C at a heating rate of 5°C / min in a muffle furnace and kept at this temperature for 2 hours.

[0121] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0122] The specific process is:

[0123] The cerium oxide nanosphere film obtained in step 2 is immersed in an anhydrous ethanol solution of hexadecyltrimethyloxysilane with a concentration of 40 g / L for modification for 15 min, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and then dried at 80° C. for 10 min to 30 min, and then a layer of perfluorosilane is self-assembled on the surface of the cerium oxide to obtain a super-hydrophobic cerium oxide nanosphere film;

[0124] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0125] The specific process is:

[0126] A mask with an aperture size of r = 50 mm is covered on the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3, and then ultraviolet light with a wavelength of 180nm to 280nm is irradiated on the unmasked area for 4 hours at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0127] like Figure 4 As shown, it can be seen intuitively from the SEM image that the microstructure of the cerium oxide super-hydrophilic / super-hydrophobic array fog-collecting film prepared by the method of the present invention is in the form of nanospheres.

[0128] Example 4

[0129] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0130] The specific process is:

[0131] Step 1.1, 5.0760 g of cerium (III) acetate hydrate was dissolved in 20 mL of anhydrous methanol, and then 3.5558 g of catalyst propionic acid was added. After sealing, the mixture was stirred at room temperature for 10 h on a magnetic stirrer and aged for 24 h to obtain a yellow-brown transparent cerium oxide sol with a concentration of 0.80 mol / L;

[0132] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dip-pulling method at a pulling speed of 3.5 mm / s;

[0133] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0134] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above process 3 times, and keep the temperature at 800°C for 2 hours for the third time; during this heat treatment process, the polymer will gradually decompose to form cerium oxide, and the cerium oxide film will be obtained as the substrate of the hydrothermal method;

[0135] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0136] The specific process is:

[0137] Step 2.1, 1.0421 g of cerium nitrate hexahydrate as a cerium source and 0.4324 g of urea as an alkali source are fully dissolved in 30 mL of deionized water, and after the solution is completely clarified, a hydrothermal reaction solution of cerium oxide with a concentration of 0.08 mol / L is obtained;

[0138] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0139] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0140] The drying temperature is 80°C and the drying time is 10-20 minutes. The annealing process is as follows: the temperature is raised to 450°C at a heating rate of 5°C / min in a muffle furnace and kept at this temperature for 2 hours.

[0141] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0142] The specific process is:

[0143] The cerium oxide nanosphere film obtained in step 2 is immersed in an anhydrous ethanol solution of vinyltrimethoxysilane with a concentration of 45 g / L for modification for 10 min, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and then dried at 80° C. for 10 min to 30 min, and then a layer of perfluorosilane is self-assembled on the surface of the cerium oxide to obtain a super-hydrophobic cerium oxide nanosphere film;

[0144] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0145] The specific process is:

[0146] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 280 nm is irradiated on the unmasked area for 5 hours at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

[0147] like Figure 5-Figure 10 The figure shows the surface morphology and element distribution of the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film prepared by the method of the present invention. It can be seen that the Ce element, O element, and C element are distributed relatively densely and evenly, indicating that a dense cerium oxide nanosphere super-hydrophilic / super-hydrophobic array fog collecting film has been prepared, in which a lattice vacancy appears in some positions of the F element, corresponding to the super-hydrophilic area obtained by deep ultraviolet light irradiation, and the rest is a super-hydrophobic area.

[0148] Example 5

[0149] Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method;

[0150] The specific process is:

[0151] Step 1.1, 5.0760 g of cerium (III) acetate hydrate was dissolved in 20 mL of anhydrous methanol, and then 3.5558 g of catalyst propionic acid was added. After sealing, the mixture was stirred at room temperature for 2 h on a magnetic stirrer and aged for 24 h to obtain a yellow-brown transparent cerium oxide sol with a concentration of 0.80 mol / L;

[0152] Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by an immersion-pulling method at a pulling speed of 4 mm / s;

[0153] Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film;

[0154] The heat treatment process is as follows: first keep the temperature at 200°C for 10 minutes, then heat from 200°C to 800°C and keep the temperature for 15 minutes, repeat the above process 3 times, and keep the temperature at 800°C for 2 hours for the third time; during this heat treatment process, the polymer will gradually decompose to form cerium oxide, and the cerium oxide film will be obtained as the substrate of the hydrothermal method;

[0155] Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film;

[0156] The specific process is:

[0157] Step 2.1, 1.0421 g of cerium nitrate hexahydrate as a cerium source and 0.4324 g of urea as an alkali source are fully dissolved in 30 mL of deionized water, and after the solution is completely clarified, a hydrothermal reaction solution of cerium oxide with a concentration of 0.08 mol / L is obtained;

[0158] Step 2.2, place the cerium oxide film obtained in step 1 in a 50 mL polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pour the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner. During this process, the volume of the reaction liquid shall not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner. Place the polytetrafluoroethylene liner in a hydrothermal autoclave and react at 100°C for 24 hours, cool to room temperature with the furnace, and take out the sample after the reaction is completed;

[0159] Step 2.3, washing the excess cerium oxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, drying and annealing the washed sample to obtain a cerium oxide nanosphere film;

[0160] The drying temperature is 60°C and the drying time is 10 to 20 minutes. The annealing process is as follows: the temperature is raised to 450°C at a heating rate of 4°C / min in a muffle furnace and kept at this temperature for 2 hours.

[0161] Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film;

[0162] The specific process is:

[0163] The cerium oxide nanosphere film obtained in step 2 is immersed in an anhydrous ethanol solution of vinyltrimethoxysilane with a concentration of 60 g / L for modification for 50 min, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and then dried at 25° C. for 10 min to 30 min, and then a layer of perfluorosilane is self-assembled on the surface of the cerium oxide to obtain a super-hydrophobic cerium oxide nanosphere film;

[0164] Step 4: Covering the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and irradiating with deep ultraviolet light to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film;

[0165] The specific process is:

[0166] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 280 nm is irradiated on the unmasked area for 8 hours at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

Claims

1. Preparation method of cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film, It is characterized in that Follow the steps below to implement it: Step 1, preparing a cerium oxide thin film on a silicon substrate by a sol-gel method; Step 2, using a hydrothermal synthesis method to immobilize nanospheres on the surface of the cerium oxide film to obtain a cerium oxide nanosphere film; Step 3: using molecular self-assembly technology to modify the cerium oxide film with a nanosphere structure on the surface to obtain a super-hydrophobic cerium oxide nanosphere film; Step 4: Cover the surface of the super-hydrophobic cerium oxide nanosphere film with masks of different specifications, and use deep ultraviolet irradiation to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

2. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, It is characterized in that The specific process of step 1 is: Step 1.1, adding cerium (III) acetate hydrate into anhydrous methanol to dissolve, then adding catalyst propionic acid, sealing, stirring, standing and aging, to obtain cerium oxide sol; Step 1.2, immersing the cleaned silicon wafer into the cerium oxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the silicon wafer by a dip-pulling method; Step 1.3, placing the sol-gel film obtained in step 1.2 into a muffle furnace for heat treatment, and cooling the furnace to obtain a cerium oxide film.

3. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 2, It is characterized in that In step 1.1, the concentration of the cerium oxide sol is 0.10 mol / L to 0.80 mol / L, and the molar ratio of cerium (III) acetate hydrate to propionic acid is 1:3; In step 1.2, the pulling speed of the immersion-pulling method is 0.5 mm / s to 4 mm / s; In step 1.3, the heat treatment process is: first keep warm at 200°C for 10 minutes, then heat from 200°C to 800°C and keep warm for 15 minutes, repeat the above treatment process 3 times, and keep warm at 800°C for 2 hours for the third time.

4. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, It is characterized in that The specific process of step 2 is: Step 2.1, using cerium nitrate hexahydrate as a cerium source and urea as an alkali source, fully dissolving them in deionized water, and after the solution is completely clarified, obtaining a cerium oxide hydrothermal reaction solution; Step 2.2, placing the cerium oxide film obtained in step 1 in a polytetrafluoroethylene liner with the film surface tilted downward at 45 degrees, and pouring the cerium oxide hydrothermal reaction liquid obtained in step 2.1 into the polytetrafluoroethylene liner, placing the polytetrafluoroethylene liner in a hydrothermal kettle for reaction, cooling to room temperature with the furnace, and taking out the sample after the reaction is completed; Step 2.3, using deionized water and anhydrous ethanol to alternately wash the excess cerium oxide nanopowder attached to the surface of the sample, and drying and annealing the washed sample to obtain a cerium oxide nanosphere film.

5. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 4, It is characterized in that In step 2.1, the concentration of the cerium oxide hydrothermal reaction solution is 0.010 mol / L to 0.080 mol / L; In step 2.2, the reaction temperature in the hydrothermal reactor is 100°C and the reaction time is 24h; In step 2.3, the drying temperature is 60°C to 80°C, and the drying time is 10min to 20min; the annealing process is: raising the temperature to 450°C in a muffle furnace at a heating rate of 3°C / min to 5°C / min and keeping it warm for 2h.

6. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, It is characterized in that The specific process of step 3 is: immersing the cerium oxide nanosphere film obtained in step 2 in a low surface energy modifier solution for modification, taking it out and washing it with anhydrous ethanol to remove the modifier remaining on the surface, and drying it to obtain a super hydrophobic cerium oxide nanosphere film.

7. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 6, It is characterized in that The concentration of the low surface energy modifier solution is 15g / L to 60g / L, the low surface energy modifier is one of octadecyltrimethyloxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, hexadecyltrimethyloxysilane, and vinyltrimethoxysilane, the solvent is anhydrous ethanol, the immersion modification time is 10min to 50min, the drying temperature is 25℃ to 80℃, and the time is 10min to 30min.

8. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, It is characterized in that The specific process of step 4 is: covering the surface of the super-hydrophobic cerium oxide nanosphere film obtained in step 3 with a mask having a specific pattern, and then irradiating the unmasked area with deep ultraviolet light at room temperature to obtain a cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film.

9. The method for preparing the cerium oxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 8, It is characterized in that The wavelength of ultraviolet light is 180nm~280nm, and the irradiation time is 3h~8h.

10. Cerium oxide super hydrophilic / super hydrophobic array fog collecting film, It is characterized in that The method is adopted as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Construction method of titanium surface micrometre-grade pattern based on ultra-hydrophilic / ultra-hydrophobic characteristic

    CN101016642A

  • Metallic aluminum bionic super-hydrophobic surface preparation method

    CN102586771A

  • Preparation method of efficient condensation hydrophilic and hydrophobic thin-film coating with multi-scale structure

    CN110372225A

  • Preparation method of cerium oxide memristor film

    CN110707211A

  • Silicon substrate super-hydrophobic surface and preparation method and application thereof

    CN111330829A

Cited By

  • Metal surface modification method, obtained modified metal and application thereof

    CN121161288A