S-waveband acceleration structure welding process
By combining segmented welding and total welding processes, combined with precise temperature control and welding process monitoring of high-temperature vacuum welding furnaces, and using high-frequency ultrasonic and laser cleaning, the stability and controllability of the S-band accelerated structure welding process is achieved, and the solution is solved The problems of unstable welding quality and insufficient controllability have improved welding quality and production efficiency.
Patent Information
- Application Number
- CN202411053507.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-05
AI Technical Summary
There are problems in the welding process of S-band accelerated structures with unstable welding quality and insufficient controllability, resulting in insufficient structural strength and sealing, making it difficult to ensure the repeatability and consistency of the welding process, affecting product quality.
Welding methods that combine segment welding and total welding processes, including the precise temperature control system and welding process monitoring system of high-temperature vacuum welding furnace, surface cleaning is used using high-frequency ultrasonic cleaning machines and non-contact laser cleaning machines, and adaptively The algorithm and feedback control mechanism dynamically adjust the heating rate and insulation time, monitor the temperature and pressure in real time, and use a high-precision helium mass spectrometer to ensure the perfection of the weld.
Improve the stability and controllability of welding quality, reduce welding defects caused by improper temperature control, ensure the formation quality of welding joints, enhance the reliability and production efficiency of the welding process, and ensure that the welding joints are fine after welding The leakage point improves the structural strength and sealing of the product.
Smart Images

Figure CN118893263A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of S-band acceleration structures, in particular to a welding process of an S-band acceleration structure. Background Art
[0002] The S-band accelerating structure is one of the core components of particle accelerators, and plays a vital role in the design and application of linear accelerators. It uses radio frequency (RF) energy to accelerate charged particles (such as electrons or protons) through changing electromagnetic fields, raising their energy to extremely high levels. "S-band" represents the frequency range in which this accelerating structure operates, which is usually between 2 and 4 GHz, and this range is within the microwave frequency band. In the manufacturing process of the S-band accelerating structure, the welding process is one of the key steps to ensure its precision performance and long-term stability. Welding not only needs to ensure the mechanical strength of the structure, but also ensure that the transmission performance of the microwave signal is not affected. Therefore, it is necessary to use special welding techniques and processes to manufacture these accelerating structures.
[0003] Although the S-band accelerating structure plays a vital role in particle accelerators, it still faces a series of challenges in its existing production and manufacturing process, especially in the welding process. First, the instability of welding quality may lead to insufficient structural strength and sealing, which is particularly critical for accelerating structures that withstand the impact of high-energy particles. Second, the controllability of the entire welding process is insufficient. Since the welding process is difficult to accurately control, the repeatability and consistency of each weld point are difficult to guarantee, which further aggravates the fluctuation of product quality. Therefore, we proposed the S-band accelerating structure welding process. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the shortcomings of the prior art, the present invention provides an S-band acceleration structure welding process, which has the advantages of stable and controllable welding quality and solves the problems of, first, the instability of welding quality, which may lead to insufficient structural strength and sealing, which is particularly critical for acceleration structures that withstand high-energy particle impacts; secondly, the insufficient controllability of the entire welding process. Since the welding process is difficult to accurately control, the repeatability and consistency of each weld point are difficult to ensure, which further aggravates the problem of product quality fluctuations.
[0006] (II) Technical solution
[0007] In order to achieve the above-mentioned purpose of stable and controllable welding quality, the present invention provides the following technical solution: S-band accelerated structural welding process, including segmented welding and total welding, the segmented welding includes the following steps:
[0008] S1. Clean the cavity and coupler until there is no oil stain and oxide layer;
[0009] S2, pre-install the cavity and the coupler respectively;
[0010] S3, filling solder in the solder tank of the pre-assembled cavity and the coupler;
[0011] S4. After checking that everything is correct, assemble the cavity and coupler separately according to the pre-installed structure;
[0012] S5. welding the cavity and the coupler separately in a high-temperature vacuum welding furnace;
[0013] S6. After the furnace is out, all welds are tested for leaks. If they are qualified, take photos and record them, clean them and store them in a drying cabinet;
[0014] The total welding comprises the following steps:
[0015] H1. Pre-install the cavity and coupler according to the tooling installation process;
[0016] H2. After pre-installation and the quality inspection department passes the inspection, disassemble the cavity and coupler and fill the solder;
[0017] H3. After the quality inspection department has passed the inspection, the welding will be started in the furnace, and after the welding is completed, the furnace will be taken out for leak detection;
[0018] H4. Check all welds for leaks, take photos and fill in forms for record;
[0019] H5. After the leak test is passed, install it on the bracket and store it in nitrogen.
[0020] Preferably, the cavity and the coupler are cleaned by a high-frequency ultrasonic cleaning machine and a non-contact laser cleaning machine. The ultrasonic cleaning machine has an operating frequency of 40kHz, a power of 1200W, and a cleaning liquid temperature that is stable at 50-60°C. The laser cleaning machine uses a pulsed laser with a wavelength of 1064nm, a pulse width of 10ns, and a power density of 10^7W / cm 2 .
[0021] Preferably, the cleaning solution comprises the following raw materials in the following weight proportions: 15% sodium alkylbenzene sulfonate, 3% sodium tripolyphosphate, 0.5% sodium benzoate and 71.5% water.
[0022] Preferably, the cavity and the coupler are welded separately by a high-temperature vacuum welding furnace, and the high-temperature vacuum welding furnace is equipped with a precise temperature control system and a welding process monitoring system.
[0023] Preferably, the precise temperature control system includes a heating rate control program and a holding time control program. The heating rate control program dynamically calculates and sets the heating rate based on the thermal conductivity and melting point data of the cavity and coupler to be welded; the holding time control program presets the holding time according to the melting characteristics of the cavity and coupler and the joint formation requirements.
[0024] Preferably, the setting range of the heating rate is 5-20°C / min, the setting range of the holding time is 5-30 minutes, and the precise temperature control system also includes a high-precision timer and a data recording module. The high-precision timer ensures the accuracy and repeatability of the holding time; the data recording module records the temperature changes and holding time during the entire welding process.
[0025] Preferably, the heating rate control program further includes an adaptive algorithm, which automatically adjusts the heating rate according to the real-time thermal response of the cavity and the coupler to optimize the welding quality; the insulation time control program further includes a feedback control mechanism, which dynamically adjusts the insulation time according to the actual formation of the welding joint.
[0026] Preferably, the welding process monitoring system includes six temperature sensors, two pressure sensors, a high-speed data acquisition card, a graphical monitoring interface and an audible and visual alarm.
[0027] Preferably, the six temperature sensors and two pressure sensors monitor the high-temperature vacuum welding furnace in real time, and monitor the temperature and pressure during the welding process in real time; and the high-speed data acquisition card collects data from the temperature sensors and pressure sensors in real time, with a sampling frequency of at least 1 Hz; the graphical monitoring interface is located outside the high-temperature vacuum welding furnace, and displays temperature parameters and pressure parameters in real time; when the temperature or pressure is abnormal, the sound and light alarm immediately notifies the operator.
[0028] Preferably, the weld is leak-checked using a high-precision helium mass spectrometer with a sensitivity of 1×10^7Pa·m^3 / s to ensure that there are no tiny leaks in the weld after welding.
[0029] (III) Beneficial effects
[0030] Compared with the prior art, the present invention provides an S-band acceleration structure welding process, which has the following beneficial effects:
[0031] 1. The S-band accelerated structural welding process, through precise temperature control system and adaptive algorithm, the heating rate and holding time in the welding process can be dynamically adjusted according to the actual thermal response, thereby ensuring the formation quality of the welded joint. This precise control reduces welding defects caused by improper temperature control and improves the stability of welding quality.
[0032] 2. The S-band accelerates the structural welding process. The welding process monitoring system ensures that the welding conditions are always in the best state by monitoring the temperature and pressure in real time. When an abnormal situation is monitored, the sound and light alarm will immediately notify the operator so that the problem can be quickly dealt with. This real-time monitoring and rapid response mechanism greatly enhances the controllability of the welding process and reduces product quality fluctuations caused by process out of control.
[0033] 3. The S-band accelerated structure welding process uses a high-frequency ultrasonic cleaning machine and a non-contact laser cleaning machine to clean the cavity and coupler to ensure the surface cleanliness before welding. The ultrasonic cleaning machine has an operating frequency of 40kHz, a power of 1200W, and a cleaning fluid temperature of 50-60°C to ensure the cleaning effect. The laser cleaning machine uses a pulsed laser with a wavelength of 1064nm, a pulse width of 10ns, and a power density of up to 10^7W / cm 2 , further ensuring the thoroughness of cleaning. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the segmented welding process of the present invention;
[0035] Figure 2 It is a schematic diagram of the overall welding process of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention and the accompanying drawings to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] See also Figure 1-2 , S-band accelerated structural welding process, including segment welding and total welding, the segment welding includes the following steps:
[0038] S1. Clean the cavity and coupler until there is no oil stain and oxide layer;
[0039] S2, pre-install the cavity and the coupler respectively;
[0040] S3, filling solder in the solder tank of the pre-assembled cavity and the coupler;
[0041] S4. After checking that everything is correct, assemble the cavity and coupler separately according to the pre-installed structure;
[0042] S5. welding the cavity and the coupler separately in a high-temperature vacuum welding furnace;
[0043] S6. After the furnace is out, all welds are tested for leaks. If they are qualified, take photos and record them, clean them and store them in a drying cabinet;
[0044] The total welding comprises the following steps:
[0045] H1. Pre-install the cavity and coupler according to the tooling installation process;
[0046] H2. After pre-installation and the quality inspection department passes the inspection, disassemble the cavity and coupler and fill the solder;
[0047] H3. After the quality inspection department has passed the inspection, the welding will be started in the furnace, and after the welding is completed, the furnace will be taken out for leak detection;
[0048] H4. Check all welds for leaks, take photos and fill in forms for record;
[0049] H5. After the leak test is passed, install it on the bracket and store it in nitrogen.
[0050] Specifically, in the segmented welding process, the cavity and the coupler are cleaned-preinstalled-solder filled-assembled-welded-leak detected respectively. After the cavity and the coupler are welded respectively, the overall welding process is carried out. The overall welding process includes preinstallation-solder filling-assembly-welding-leak detected. In the segmented welding process and the overall welding process, the equipment used in each processing step is the same.
[0051] Furthermore, the cavity and coupler are cleaned by a high-frequency ultrasonic cleaning machine and a non-contact laser cleaning machine. The ultrasonic cleaning machine operates at a frequency of 40kHz, a power of 1200W, and a cleaning liquid temperature is stabilized at 50-60°C. The laser cleaning machine uses a pulsed laser with a wavelength of 1064nm, a pulse width of 10ns, and a power density of 10^7W / cm 2 .
[0052] Specifically, in the segmented welding process, the cleaning process of the cavity and the coupler is as follows: first, place the cavity and the coupler inside a high-frequency ultrasonic cleaning machine and immerse them in a cleaning solution to remove surface oil stains; then use a high-frequency ultrasonic cleaning machine to perform ultrasonic cleaning to remove deep dirt; then use a non-contact laser cleaning machine to perform laser cleaning to remove tiny particles; and finally dry them.
[0053] Furthermore, the cleaning solution comprises the following raw materials in the following weight proportions: 15% sodium alkylbenzene sulfonate, 3% sodium tripolyphosphate, 0.5% sodium benzoate and 71.5% water.
[0054] Specifically, sodium alkylbenzene sulfonate, as a surfactant, helps to reduce the surface tension of water, allowing the cleaning fluid to better penetrate into the surface of the cavity and coupler, improving the cleaning efficiency. In addition, it helps to emulsify grease and dirt, making it easier for them to be carried away by the cleaning fluid; sodium tripolyphosphate can form complexes with metal ions in water to prevent re-contamination of the metal surface, while increasing the alkalinity of the cleaning fluid, helping to remove grease and mineral deposits; sodium benzoate has an antiseptic effect, which can extend the service life of the cleaning fluid, prevent the growth of microorganisms, and keep the cleaning fluid clean and stable; water, as a solvent, is the most important component in the cleaning fluid, helps to dissolve other ingredients, and is the main medium in the cleaning process.
[0055] Furthermore, the cavity and the coupler are welded separately by a high-temperature vacuum welding furnace, and the high-temperature vacuum welding furnace is equipped with a precise temperature control system and a welding process monitoring system.
[0056] Furthermore, the precise temperature control system includes a heating rate control program and a holding time control program. The heating rate control program dynamically calculates and sets the heating rate based on the thermal conductivity and melting point data of the cavity and coupler to be welded; the holding time control program presets the holding time according to the melting characteristics of the cavity and coupler and the joint formation requirements.
[0057] Specifically, the precise temperature control system uses the heating rate control program to dynamically calculate and set the heating rate based on the thermal conductivity and melting point of the material, ensuring that the welding material is heated under optimal conditions and avoiding overheating or unevenness, thereby improving the welding quality. The insulation time control program presets the insulation time based on the material melting characteristics and joint formation requirements to ensure that the welded joint is uniform and stable. This precise temperature control significantly improves the consistency and reliability of welding, reduces material waste, improves production efficiency, and enhances the safety of the welding process.
[0058] Furthermore, the setting range of the heating rate is 5-20°C / min, the setting range of the holding time is 5-30 minutes, and the precise temperature control system also includes a high-precision timer and a data recording module. The high-precision timer ensures the accuracy and repeatability of the holding time; the data recording module records the temperature changes and holding time during the entire welding process.
[0059] Specifically, the precise temperature control system with a heating rate set at 5-20℃ / min and a holding time set at 5-30 minutes provides fine temperature control for S-band accelerated structure welding, ensuring the quality and consistency of the welding process. This wide range of heating rate and holding time settings allows the welding process to adapt to different material properties and welding requirements, and realizes customized welding. The addition of a high-precision timer ensures the accuracy and repeatability of the holding time, thereby avoiding welding defects caused by improper time control. At the same time, the recording function of the data recording module provides detailed temperature change and holding time data for the welding process, which are crucial for subsequent quality analysis, process optimization and problem diagnosis.
[0060] Furthermore, the heating rate control program further includes an adaptive algorithm, which automatically adjusts the heating rate and optimizes the welding quality according to the real-time thermal response of the cavity and the coupler; the insulation time control program further includes a feedback control mechanism, which dynamically adjusts the insulation time according to the actual formation of the welding joint.
[0061] Specifically, the adaptive algorithm can automatically adjust the heating rate according to the real-time thermal response of the cavity and the coupler, which means that the temperature changes during the welding process can be monitored and optimized in real time, thereby reducing errors caused by human factors and improving welding quality. At the same time, the feedback control mechanism in the insulation time control program can dynamically adjust the insulation time according to the actual formation of the welded joint to ensure the uniformity and stability of the welded joint. This intelligent temperature control not only improves the accuracy and consistency of welding, but also enhances the flexibility and adaptability of the production process.
[0062] Furthermore, the welding process monitoring system includes six temperature sensors, two pressure sensors, a high-speed data acquisition card, a graphical monitoring interface and an audible and visual alarm.
[0063] Furthermore, the six temperature sensors and two pressure sensors monitor the high-temperature vacuum welding furnace in real time, and monitor the temperature and pressure during the welding process in real time; and the high-speed data acquisition card collects data from the temperature sensors and pressure sensors in real time, with a sampling frequency of at least 1 Hz; the graphical monitoring interface is located outside the high-temperature vacuum welding furnace, and displays temperature parameters and pressure parameters in real time; when the temperature or pressure is abnormal, the sound and light alarm immediately notifies the operator.
[0064] Specifically, the deployment of six temperature sensors and two pressure sensors realizes real-time monitoring of the environment inside the welding furnace and ensures precise control of temperature and pressure during the welding process. The high-speed data acquisition card ensures the real-time and continuity of data collection with a sampling frequency of at least 1 Hz, providing detailed data support for the welding process. The setting of the graphical monitoring interface enables operators to intuitively observe and analyze the temperature and pressure changes during the welding process, improving the convenience and intuitiveness of the operation. Most importantly, the integration of sound and light alarms provides instant feedback for safety monitoring. Once an abnormality is detected, the operator can be quickly notified to take measures, effectively preventing potential welding defects and safety risks. Overall, this monitoring system not only improves the accuracy and reliability of the welding process through intelligent and automated monitoring methods, but also greatly enhances the safety and efficiency of the production process.
[0065] Furthermore, in S6, the weld is leaked by using a high-precision helium mass spectrometer with a sensitivity of 1×10^7Pa·m^3 / s to ensure that there are no tiny leaks in the weld after welding.
[0066] Specifically, using a high-precision helium mass spectrometer leak detector with a sensitivity of up to 1×10^7Pa·m^3 / s to detect welds can detect extremely small leaks, even tiny defects that are difficult for the human eye to detect. These potential defects can be discovered and repaired in time to ensure the perfect sealing of the welded joints. In addition, the application of this leak detection technology also improves the reliability of the production process, reduces rework and scrap rates caused by leaks, and improves production efficiency.
[0067] In summary, the S-band accelerated structural welding process, through a precise temperature control system and adaptive algorithm, the heating rate and holding time during the welding process can be dynamically adjusted according to the actual thermal response, thereby ensuring the formation quality of the welded joint. This precise control reduces welding defects caused by improper temperature control and improves the stability of welding quality.
[0068] In addition, the S-band accelerates the structural welding process. The welding process monitoring system ensures that the welding conditions are always in the best state by monitoring the temperature and pressure in real time. When an abnormal situation is monitored, the sound and light alarm will immediately notify the operator so that the problem can be quickly dealt with. This real-time monitoring and rapid response mechanism greatly enhances the controllability of the welding process and reduces product quality fluctuations caused by process out of control.
[0069] In addition, the S-band accelerated structural welding process uses a high-frequency ultrasonic cleaning machine and a non-contact laser cleaning machine to clean the cavity and coupler, ensuring the surface cleanliness before welding. The ultrasonic cleaning machine has an operating frequency of 40kHz, a power of 1200W, and a cleaning fluid temperature of 50-60°C to ensure the cleaning effect. The laser cleaning machine uses a pulsed laser with a wavelength of 1064nm, a pulse width of 10ns, and a power density of up to 10^7W / cm 2 , further ensuring the thoroughness of cleaning and solving the problems of, first, the instability of welding quality, which may lead to insufficient structural strength and sealing, which is particularly critical for accelerating structures that withstand high-energy particle impacts. Secondly, the lack of controllability of the entire welding process. Since the welding process is difficult to accurately control, the repeatability and consistency of each weld point are difficult to guarantee, which further aggravates the problem of product quality fluctuations.
[0070] The relevant modules involved in this system are all hardware system modules or functional modules that combine computer software programs or protocols with hardware in the prior art. The computer software programs or protocols involved in the functional modules are themselves technologies that are well known to those skilled in the art and are not improvements of this system. The improvements of this system are the interaction or connection relationships between the modules, that is, improvements to the overall structure of the system to solve the corresponding technical problems to be solved by this system.
[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. S-band accelerated structural welding process, including segment welding and total welding, characterized in that: The segmented welding comprises the following steps: S1. Clean the cavity and coupler until there is no oil stain and oxide layer; S2, pre-install the cavity and the coupler respectively; S3, filling solder in the solder tank of the pre-assembled cavity and the coupler; S4. After checking that everything is correct, assemble the cavity and coupler separately according to the pre-installed structure; S5. welding the cavity and the coupler separately in a high-temperature vacuum welding furnace; S6. After the furnace is out, all welds are tested for leaks. If they are qualified, take photos and record them, clean them and store them in a drying cabinet; The total welding comprises the following steps: H1. Pre-install the cavity and coupler according to the tooling installation process; H2. After pre-installation and the quality inspection department passes the inspection, disassemble the cavity and coupler and fill the solder; H3. After the quality inspection department has passed the inspection, the welding will be started in the furnace, and after the welding is completed, the furnace will be taken out for leak detection; H4. Check all welds for leaks, take photos and fill in forms for record; H5. After the leak test is passed, install it on the bracket and store it in nitrogen.
2. The S-band acceleration structure welding process according to claim 1 is characterized in that: In S1, the cavity and the coupler are cleaned by a high-frequency ultrasonic cleaning machine and a non-contact laser cleaning machine. The ultrasonic cleaning machine has an operating frequency of 40kHz, a power of 1200W, and a cleaning liquid temperature that is stable at 50-60°C. The laser cleaning machine uses a pulsed laser with a wavelength of 1064nm, a pulse width of 10ns, and a power density of 10^7W / cm 2 .
3. The S-band acceleration structure welding process according to claim 2 is characterized in that: The cleaning solution comprises the following raw materials in proportion by weight: 15% sodium alkylbenzene sulfonate, 3% sodium tripolyphosphate, 0.5% sodium benzoate and 71.5% water.
4. The S-band acceleration structure welding process according to claim 1, characterized in that: In S5, the cavity and the coupler are welded separately by a high-temperature vacuum welding furnace, and the high-temperature vacuum welding furnace is equipped with a precise temperature control system and a welding process monitoring system.
5. The S-band acceleration structure welding process according to claim 4 is characterized in that: The precise temperature control system includes a heating rate control program and a holding time control program. The heating rate control program dynamically calculates and sets the heating rate based on the thermal conductivity and melting point data of the cavity and the coupler to be welded; the holding time control program presets the holding time according to the melting characteristics of the cavity and the coupler and the joint formation requirements.
6. The S-band acceleration structure welding process according to claim 5, characterized in that: The setting range of the heating rate is 5-20°C / min, the setting range of the holding time is 5-30 minutes, and the precise temperature control system also includes a high-precision timer and a data recording module. The high-precision timer ensures the accuracy and repeatability of the holding time; the data recording module records the temperature changes and holding time during the entire welding process.
7. The S-band acceleration structure welding process according to claim 5, characterized in that: The heating rate control program further includes an adaptive algorithm that automatically adjusts the heating rate to optimize the welding quality according to the real-time thermal response of the cavity and the coupler; the insulation time control program further includes a feedback control mechanism that dynamically adjusts the insulation time according to the actual formation of the welding joint.
8. The S-band acceleration structure welding process according to claim 4, characterized in that: The welding process monitoring system includes six temperature sensors, two pressure sensors, a high-speed data acquisition card, a graphical monitoring interface and an audible and visual alarm.
9. The S-band acceleration structure welding process according to claim 8, characterized in that: The six temperature sensors and two pressure sensors monitor the high-temperature vacuum welding furnace in real time, and monitor the temperature and pressure during the welding process in real time; the high-speed data acquisition card collects data from the temperature sensors and pressure sensors in real time, with a sampling frequency of at least 1 Hz; the graphical monitoring interface is located outside the high-temperature vacuum welding furnace, and displays temperature parameters and pressure parameters in real time; when the temperature or pressure is abnormal, the sound and light alarm immediately notifies the operator.
10. The S-band acceleration structure welding process according to claim 1, characterized in that: In S6, a high-precision helium mass spectrometer leak detector with a sensitivity of 1×10^7Pa·m^3 / s is used to detect leaks in the weld to ensure that there are no tiny leaks in the weld after welding.