Method for preparing metal plate with reverse gradient structure based on friction stir welding
The preparation of anti-gradient structural metal sheets through friction stir welding technology solved the problem of insufficient compatibility with strength and plasticity and low processing efficiency of gradient structural materials, achieved low cost and efficient improvement of mechanical properties and fatigue resistance improvement, and expanded the application Scene.
Patent Information
- Application Number
- CN202411217937.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-05
AI Technical Summary
The existing gradient structure materials have shortcomings in strength and plastic compatibility, especially in wetland environments such as oceans and lakes, and have insufficient fatigue resistance. The processing methods are inefficient and costly, making it difficult to meet the needs of diversified mechanical properties.
Friction stir welding technology is adopted to generate heat by rotating the stirring head with the surface of the metal sheet by high-speed rotation, adjusting the stirring rate and feeding speed, realizing the recrystallization of ultrafine crystals/nano crystals, forming an inverse gradient of surface coarse crystals and fine crystals in the core. The structure and grain size are distributed radially, and metal sheets with excellent mechanical properties are prepared.
The preparation of anti-gradient structure metal sheets with low cost and controllable processes is realized, which improves the comprehensive mechanical properties, corrosion resistance and fatigue resistance of the material, expands the application scenarios, and avoids the problems of surface structure unevenness and high equipment costs. .
Smart Images

Figure CN118893299A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heterogeneous metal materials, and in particular relates to a method for preparing a metal plate with an anti-gradient structure based on friction stir welding. Background Art
[0002] In engineering applications, the problem of the incompatibility of strength and toughness of metal materials has long plagued practical applications. Generally, traditional metal materials show an inverted relationship of "strength increases, plasticity decreases" in strength and plasticity, which greatly limits the application scope of metal materials. The research on gradient structured metals provides a feasible material design idea. Nano-sizing the metal surface through surface machining can improve the strength of the material, and the coarse grains in the core maintain the plasticity of the material. This gradient structure of ultrafine grains / nano-crystals on the surface and coarse grains in the core obtains comprehensive mechanical properties that match the strength and plasticity of the material. However, the relatively small thickness of the fine grain layer on the surface of the existing gradient material has limited effect on improving strength, and it is difficult to meet the use requirements of different mechanical performance requirements. In addition, although the gradient structure material has improved strength after surface refinement, due to plastic deformation, there are often a large number of high-energy and high-stress areas on the surface, such as grain boundaries and high-density dislocations. These areas are the priority corrosion areas of the material, which greatly limits the use of the material in scenes such as oceans, lakes, and wetlands.
[0003] Changing the organizational structure characteristics of the gradient structure to form an anti-gradient structure with soft coarse crystals on the surface and hard fine crystals in the core can, on the one hand, better control the fine crystal volume fraction and achieve diversified and large-scale regulation of the mechanical properties of the material; on the other hand, it reduces the disadvantages of material surface damage caused by large plastic deformation. The surface coarse crystals can effectively reduce the generation of external cracks and avoid the reduction of corrosion resistance, thereby expanding the application of gradient structure materials in environments such as oceans, lakes, and wetlands. In addition, the design of anti-gradient structure materials can effectively improve the material's fatigue resistance, and is expected to be expanded in bridges, building structures, and heavy machinery.
[0004] The methods for processing anti-gradient structures in the prior art include: gradient cold rolling, laser surface treatment and induction heating. However, the laser spot area of laser surface treatment is small, and the processing efficiency is low. When processing a large area, multiple overlaps are likely to cause periodic fluctuations in the surface organization and performance, thereby causing instability in its microstructure and mechanical properties. Gradient cold rolling is a cold rolling technology for processing wires with circular cross-sections. Under moderate deformation conditions, the core of the rod is refined to the nanoscale, while the edge area is still a coarse-grained structure. Although this method can avoid the instability of surface organization and performance caused by laser surface treatment, due to the small difference in rod thickness, its deformation process often only triggers a small amount of dynamic recrystallization behavior, and it is difficult to obtain an anti-gradient structure with significant differences. Induction heating can only heat the material as a whole, so its flexibility and directionality are poor, the equipment cost is high, and the professional technology required for control and maintenance is large. The heating process may cause uneven heating. At the same time, high-frequency and high-voltage currents often bring safety hazards in actual applications. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an inverse gradient metal material with low cost and good controllability. Specifically, the stirring head rotates at high speed to rub the surface of the plate, and the stirring head is inserted into the surface of the plate under the action of pressure, so that the temperature rises to cause plastic softening of the surface of the plate, and the stirring rate and feeding speed of the stirring head are regulated to cause the ultrafine crystals / nano crystals to recover and recrystallize, thereby obtaining a metal plate with coarse crystals on the surface, fine crystals in the core, and the grain size distributed along the radial inverse gradient as a whole.
[0006] The technical solution to achieve the purpose of the present invention is: a method for preparing a metal sheet with an anti-gradient structure based on friction stir welding, comprising the following steps:
[0007] Step (1): preparing an ultrafine crystal / nanocrystalline plate with a grain size of 10 nm to 5 μm;
[0008] Step (2): The surface of the plate obtained in step (1) is subjected to stir friction processing with a shoulder radius of 5 to 15 mm, a stirring head rotation speed of 600 to 2000 r / min, a processing speed of 30 mm / min to 200 mm / min, and a shoulder reduction of 0.1 mm to 0.3 mm to obtain a metal plate with an anti-gradient structure in which the surface has a coarse grain / fine grain area of 5 μm to 50 μm, the core is still ultrafine grain / nano grain, and the grain size decreases from the surface layer to the inner layer.
[0009] Furthermore, the ultrafine-grained / nanocrystalline plate prepared in step (1) is made of magnesium alloy, aluminum alloy, titanium alloy or steel.
[0010] Furthermore, the preparation method in step (1) is specifically: high temperature multi-directional forging is used for preliminary refinement, and then room temperature rolling is used until an ultrafine grain / nanocrystalline sheet is obtained.
[0011] Furthermore, in step (1), the temperature of the high-temperature multi-directional forging does not exceed 900° C., and the rolling reduction is 50% to 95%.
[0012] Furthermore, a stirring head shoulder is arranged below the stirring head, and the stirring head shoulder is cylindrical. During the friction stirring processing, the shoulder contacts with the plate to be processed.
[0013] Furthermore, the stirring head is made of martensitic stainless steel, medium carbon steel, high carbon steel, tool steel or high temperature alloy.
[0014] Furthermore, the heat input calculation formula for friction stir welding is as follows:
[0015]
[0016] where k m is a constant coefficient, n and v are the stirring head speed and welding speed respectively. By changing the stirring head speed n and the welding speed v, the thickness of the anti-gradient structure can be quantitatively controlled.
[0017] Furthermore, the friction stir zone covers the entire surface of the plate, or the horizontal distance between the axes of the friction stir processing of adjacent passes is any multiple of the diameter of the stirring head.
[0018] A metal plate with an inverse gradient structure is prepared by the above method.
[0019] Compared with the prior art, the present invention has the following significant advantages:
[0020] (1) It does not require special environments such as vacuum, specific temperature, electric field, magnetic field, etc. The preparation process is simple, the process is controllable, and the production cost is low;
[0021] (2) This method uses a solid-state reciprocating processing method to avoid uneven surface structure of the plate during the processing process, and the performance is stable; the processing process only generates heat through the friction between the stirring head and the workpiece, and does not involve chemical treatment, which is a green processing technology;
[0022] (3) This method can be used to design stir friction parameters in a diversified manner, and has greater microstructure design directionality and flexibility;
[0023] (4) The anti-gradient structural material prepared by this method has excellent comprehensive mechanical properties, good corrosion resistance, and good fatigue resistance, which expands the application scenarios of gradient materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the processing of obtaining ultrafine-grained / nanocrystalline plates by refining grains through multi-directional forging combined with rolling.
[0025] Figure 2It is a schematic diagram of the processing of preparing metal plates of anti-gradient structural materials based on stir friction welding in the present invention.
[0026] Figure 3 The schematic diagram of the stirring head structure of the friction stirring process of the present invention, wherein 1 is the stirring head; 2 is the shoulder of the welding stirring head without a stirring needle.
[0027] Figure 4 Schematic diagrams of three different stir friction processing methods; (a) is a stir friction layer covering the entire plate surface, (b) is a plate surface where the horizontal distance between the processing axes of the stir friction zone is twice the diameter of the stirring head, and (c) is a plate surface where the horizontal distance between the processing axes of the stir friction zone is an arbitrary multiple of the stirring head diameter and has a non-uniform coarse grain zone.
[0028] Figure 5 Schematic diagram of the evolution of the microstructure of the ultrafine-grained / nanocrystalline plate along the rolling direction RD and the transverse direction TD before and after friction stir processing, where (a) is a schematic diagram of the microstructure of the unprocessed coarse-grained sample along the rolling direction RD, (b) is a schematic diagram of the microstructure of the ultrafine-grained / nanocrystalline structure along the rolling direction RD after multi-directional forging combined with rolling deformation, and (c1) is a schematic diagram of the microstructure of the ultrafine-grained / nanocrystalline structure along the rolling direction RD after multi-directional forging combined with rolling deformation. Figure 4 (a) Schematic diagram of the microstructure along the rolling direction RD after friction stir treatment, Figure (c2) Figure 4 (b) Schematic diagram of the microstructure along the rolling direction RD after friction stir treatment. Figure (c3) is a schematic diagram of the microstructure along the rolling direction RD after friction stir treatment. Figure 4 (c) Schematic diagram of the microstructure along the transverse direction TD of the rolled surface after friction stir treatment. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with the accompanying drawings.
[0030] like Figure 1-5 As shown, a method for preparing a metal sheet with an inverse gradient structure based on friction stir welding is based on a friction stir heating process, which relies on the mutual friction between the stirring head and the ultrafine crystal / nano crystal sheet to generate heat, so that the surface of the sheet undergoes plastic softening, and the rotation rate and feed speed of the stirring head are regulated to cause the ultrafine crystal / nano crystal to recover and recrystallize, thereby obtaining a metal sheet with a complex coarse grain distribution on the outside, fine grains in the center, and a grain size inverse gradient distribution along the radial direction. When the welding stirring head shaft shoulder 2 rotates at a high speed and contacts the substrate, the substrate surface heats up rapidly.
[0031] The specific steps of this method are as follows:
[0032] Step (1): Preparation of ultrafine grain / nanocrystalline sheet: multi-directional forging is performed on the base material, the size of the base material is within 300 mm×300 mm×50 mm, and its grain structure is initially refined, and then cold-rolled at room temperature to shape it into a sheet, and the grains are further refined to achieve ultrafine grain / nanocrystalline, wherein the multi-directional forging temperature is adjusted from room temperature to a maximum of 900°C according to the plastic deformation capacity and strength difference of the processed material, and the rolling pressure is 50% to 95%;
[0033] Step (2): clamping the raw material: clamping the rolled plate on the workbench using a clamp;
[0034] Step (3): Process the rolled plate with a stirring friction head, perform stirring friction processing along the surface of the rolled plate, and roughen the surface structure by frictional heat generation. The stirring friction processing can process the entire upper and lower surfaces of the material, or can be performed at intervals. Stirring friction can be performed along the RD direction or along the TD direction of the rolled plate. The rotation speed of the stirring head is 600-2000r / min, the forward speed of the stirring head is 30-200mm / min, the pressure of the stirring head is 0.1-0.3mm, and the stirring head performs multiple passes along the rolled surface of the plate, controlling the horizontal distance between the two parallel processing axes to obtain a plate whose surface is completely covered by the stirring layer or a plate whose surface is covered by the stirring layer at intervals;
[0035] Step (4): turning over the rolled plate after the friction stir processing, re-clamping, and performing friction stir processing on the turned rolled plate according to the direction and position of step (3);
[0036] Repeat step (4) 2 to 4 times, perform surface finishing treatment on the plate obtained after processing, grind it, and remove the burrs of stir friction welding to obtain the anti-gradient material.
[0037] Example 1
[0038] (1) Selecting AZ31 magnesium alloy plates with a plate size of 70 mm × 50 mm × 10 mm; performing multi-directional forging to initially refine the AZ31 magnesium alloy plates, and then cold rolling the materials at room temperature until ultrafine grains are obtained;
[0039] (2) The rolled plate is clamped on a workbench using a fixture, and the rolled substrate is subjected to friction stir treatment. The rotation speed of the friction stir welding is set to 1200 r / min, the forward speed is 60 mm / min, the shoulder axis downward pressure is 0.1 mm, and multiple passes of friction stir welding are performed along the rolling direction, so that the horizontal distance between two parallel adjacent processing axes is the diameter of the stirring head until the entire plate surface is fully covered;
[0040] (3) turning over the rolled plate after the friction stir processing, re-clamping, and performing friction stir processing on the turned rolled plate according to the direction and position of step (3);
[0041] (4) Repeat step (3) 2 to 4 times, perform surface finishing treatment on the plate obtained after processing, grind it, and remove the burrs of stir friction welding to obtain the reverse gradient material.
[0042] Example 2
[0043] (1) Selecting a 6061 aluminum alloy plate with a plate size of 100 mm × 70 mm × 6 mm; performing multi-directional forging to perform preliminary refinement on the 6061 aluminum alloy plate, and then performing room temperature cold rolling on the material until ultrafine grains are obtained;
[0044] (2) The rolled plate is clamped on a workbench using a fixture, and the rolled substrate is subjected to friction stir welding. The rotation speed of the friction stir welding is set to 1000 r / min, the forward speed is set to 30 mm / min, the shoulder axis downward pressure is set to 0.2 mm, and multiple passes of friction stir welding are performed along the rolling direction so that the horizontal distance between two parallel adjacent processing axes is twice the diameter of the stirring head;
[0045] (3) turning over the rolled plate after the friction stir processing, re-clamping, and performing friction stir processing on the turned rolled plate according to the direction and position of step (3);
[0046] (4) Repeat step (3) 2 to 4 times, perform surface finishing treatment on the plate obtained after processing, grind it, and remove the burrs of stir friction welding to obtain the reverse gradient material.
[0047] Example 3
[0048] (1) A 6082 aluminum alloy plate with a plate size of 150 mm × 100 mm × 5 mm was selected; the 6082 aluminum alloy plate was subjected to multi-directional forging for preliminary refinement, and then the material was cold rolled at room temperature until ultrafine grains were obtained;
[0049] (2) The rolled plate was clamped on the workbench using a fixture, and the rolled substrate was subjected to friction stir treatment. The rotation speed of the friction stir welding was set to 900 r / min, the forward speed was 50 mm / min, and the shoulder axis downward pressure was 0.1 mm. Multiple friction stir welding was performed along the rolling direction so that the horizontal distance between two parallel adjacent processing axes was twice the diameter of the stirring head. When processing the four friction stir zones on both sides of the central axis of the plate surface, the rotation speed of the friction stir welding was changed to 1200 r / min, the forward speed was 30 mm / min, and the shoulder axis downward pressure was 0.2 mm.
[0050] (3) turning over the rolled plate after the friction stir processing, re-clamping, and performing friction stir processing on the turned rolled plate according to the direction and position of step (3);
[0051] (4) Repeat step (3) 2 to 4 times, perform surface finishing treatment on the plate obtained after processing, grind it, and remove the burrs of stir friction welding to obtain the reverse gradient material.
[0052] Example 4
[0053] (1) A 304 stainless steel sheet with a size of 120 mm × 80 × 6 mm was selected, the 304 stainless steel sheet was subjected to multi-directional forging for preliminary refinement, and then the material was cold rolled at room temperature until it became nanocrystalline;
[0054] (2) The rolled plate is clamped on a workbench using a fixture, and the rolled substrate is subjected to friction stir welding. The rotation speed of the friction stir welding is set to 1500 r / min, the forward speed is 50 mm / min, the shoulder axis downward pressure is 0.3 mm, and multiple passes of friction stir welding are performed along the rolling direction, so that the horizontal distance between two parallel adjacent processing axes is the diameter of the stirring head until the entire plate surface is fully covered;
[0055] (3) turning over the rolled plate after the friction stir processing, re-clamping, and performing friction stir processing on the turned rolled plate according to the direction and position of step (3);
[0056] (4) Repeat step (4) 2 to 4 times, perform surface finishing treatment on the plate obtained after processing, grind it, and remove the burrs of stir friction welding to obtain the reverse gradient material.
Claims
1. A method for preparing a metal sheet with an anti-gradient structure based on friction stir welding. It is characterized in that The steps include: Step (1): preparing an ultrafine crystal / nanocrystalline plate with a grain size of 10 nm to 5 μm; Step (2): The surface of the plate obtained in step (1) is subjected to stir friction processing with a shoulder radius of 5 to 15 mm, a stirring head rotation speed of 600 to 2000 r / min, a processing speed of 30 mm / min to 200 mm / min, and a shoulder reduction of 0.1 mm to 0.3 mm to obtain a metal plate with an anti-gradient structure in which the surface has a coarse grain / fine grain area of 5 μm to 50 μm, the core is still ultrafine grain / nano grain, and the grain size decreases from the surface layer to the inner layer.
2. The method according to claim 1, It is characterized in that The material of the ultrafine crystal / nano crystal plate prepared in step (1) is magnesium alloy, aluminum alloy, titanium alloy or steel.
3. The method according to claim 2, It is characterized in that The preparation method in step (1) is specifically: high-temperature multi-directional forging is used for preliminary refinement, and then room temperature rolling is used until an ultrafine grain / nanocrystalline sheet is obtained.
4. The method according to claim 3, It is characterized in that In step (1), the temperature of high-temperature multi-directional forging does not exceed 900° C., and the rolling reduction is 50% to 95%.
5. The method according to claim 4, It is characterized in that The stirring head shoulder is arranged below the stirring head, and the stirring head shoulder is cylindrical. During the friction stirring processing, the shoulder contacts with the plate to be processed.
6. The method according to claim 5, It is characterized in that The material of the stirring head is martensitic stainless steel, medium carbon steel, high carbon steel, tool steel or high temperature alloy.
7. The method according to claim 6, It is characterized in that The heat input calculation formula for friction stir welding is as follows: where k m is a constant coefficient, n and v are the stirring head speed and welding speed respectively. By changing the stirring head speed n and the welding speed v, the thickness of the anti-gradient structure can be quantitatively controlled.
8. The method according to claim 7, It is characterized in that The friction stir zone covers the entire surface of the plate, or the horizontal distance between the friction stir processing axes of adjacent passes is any multiple of the stirring head diameter.
9. An anti-gradient structural metal sheet, It is characterized in that The method is prepared by any one of claims 1 to 8.
Citation Information
Cited By
Method for preparing gradient nanometer structure in as-cast aluminum-lithium alloy through friction stir processing and product
CN120967264A