Corrosion-resistant welding wire and preparation method thereof

By adding copper to the nickel-based alloy and adopting a specific smelting process, a corrosion-resistant welding wire was prepared, which solved the problem of insufficient corrosion resistance of existing nickel-based welding wire in high-temperature chloride ions and strong oxidative acidic environments, and achieved Higher tensile strength and hardness meet the corrosion needs of high-temperature chloride ions and strong oxidative acidic environments.

CN118893365APending Publication Date: 2024-11-05CHONGQING SANFENG COVANTA ENVIRONMENTAL IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410950490.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing nickel-based welding wires have insufficient corrosion resistance in high-temperature chloride ions and strong oxidative acid environments, and cannot meet the corrosion resistance needs of high-temperature chloride ions and strong oxidative acid environments.

Method used

A new corrosion-resistant welding wire is prepared by adding copper to a nickel-based alloy through induction furnace smelting, electroslag remelting, forging, annealing, cold drawing and other processes. Its chemical composition is 23%≤Cr≤25%, Fe≤ 5%, 6%≤Mo≤8%, 3%≤Cu≤4.5%, 3%≤W≤5%, C≤0.1%, Si≤0.5%, Mn≤0.5%, P≤0.02%, S≤0.015 %, the balance is Ni and ≥51%, and multiple cold drawing and intermediate annealing treatments were performed to produce welding wires with higher tensile strength and hardness.

Benefits of technology

The corrosion-resistant welding wire shows better corrosion resistance in high-temperature chloride ions, molten salts, sulfur anhydrides, oxidation and other corrosion environments, reduces stress corrosion sensitivity, and meets the corrosion needs of high-temperature chloride ions and strong oxidative acidic environments .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947084030000031
    Figure BDA0004947084030000031
  • Figure BDA0004947084030000032
    Figure BDA0004947084030000032
Patent Text Reader

Abstract

The invention belongs to the technical field of welding materials, and relates to a corrosion-resistant welding wire and a preparation method thereof, and the corrosion-resistant welding wire comprises the following alloy components in percentage by mass: 23%-25% of Cr, 5%-5% of Fe, 6%-8% of Mo, 3%-4.5% of Cu, 3%-5% of W, 0.1%-0.1% of C, 0.5%-0.5% of Si, 0.5%-0.5% of Mn, 0.02%-0.02% of P, 0.015%-0.015% of S and the balance of Ni and less than or equal to 0.5% of impurities. The method comprises the following steps: weighing different types of alloy elements in proportion, uniformly mixing, and smelting in an induction furnace to obtain a primary master alloy ingot; carrying out electroslag remelting or vacuum self-consumption to obtain a secondarily refined master alloy ingot, carrying out heat preservation at 1000-1080 DEG C for 1-2.5 h, and forging to obtain a forged square billet; and the forged square billet is hot-rolled into a steel wire rod with the specified size, and the welding wire with the specified size is obtained after annealing treatment, rough wire drawing, continuous cold drawing and intermediate annealing processes. Compared with an existing nickel-based welding wire, the corrosion-resistant welding wire has better corrosion resistance, and the problem that an existing nickel-based welding wire cannot meet the corrosion resistance requirement in the high-temperature chloride ion and strong-oxidizing-property acid environment is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding materials and relates to a corrosion-resistant welding wire and a preparation method thereof. Background Art

[0002] With the development of industry and the shortage of renewable resources and energy, equipment is required to be more and more tolerant to corrosive environments. For example, oil pipelines, caustic soda furnaces, industrial acid production, thermal power generation units, waste incineration generation units, and hazardous waste treatment all have varying degrees of corrosion. In waste incineration power generation projects, equipment is required to be resistant to high-temperature chloride ion and molten salt corrosion, and in thermal power generation units, equipment is required to be resistant to sulfuric anhydride corrosion and high-temperature oxidation corrosion. In industrial sulfuric acid production, equipment is required to be resistant to sulfuric acid of different concentrations at different temperatures.

[0003] A large number of nickel-based welding wires are used as corrosion-resistant layers in various corrosion-resistant environments, especially environments that require resistance to chloride ion corrosion, such as Ni-Cr-Fe, Ni-Cr-Mo, Ni-Cr-Mo-Nb, Ni-Cr-Mo-W and other nickel-based welding wires. However, their corrosion resistance is weakened in high temperature and strongly oxidizing acidic environments, resulting in the existing nickel-based welding wires being unable to meet the corrosion resistance requirements in high temperature chloride ion and strongly oxidizing acidic environments. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a corrosion-resistant welding wire and a preparation method thereof, which has better corrosion resistance than the existing nickel-based welding wire, so as to solve the problem that the existing nickel-based welding wire cannot meet the corrosion resistance requirements in high-temperature chloride ion and strong oxidizing acidic environments.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A corrosion-resistant welding wire consists of the following components in parts by mass: 23%≤Cr≤25%, Fe≤5%, 6%≤Mo≤8%, 3%≤Cu≤4.5%, 3%≤W≤5%, C≤0.1%, Si≤0.5%, Mn≤0.5%, P≤0.02%, S≤0.015%, the balance is Ni and ≥51%, and impurities are ≤0.5%.

[0007] A method for preparing a corrosion-resistant welding wire comprises the following steps:

[0008] According to the above alloy composition, different types of alloy elements are weighed according to the proportion, mixed evenly, and then smelted in an induction furnace to obtain a primary master alloy ingot;

[0009] After electroslag remelting or vacuum self-consumption, a secondary refined master alloy ingot is obtained, which is then forged after being kept at 1000-1080°C for 1-2.5 hours to obtain a forged square billet;

[0010] The forged square billet is hot rolled into a wire rod of a specified size, and then the welding wire of the specified size is obtained after annealing, rough drawing, continuous cold drawing and intermediate annealing.

[0011] Furthermore, the tensile strength of the corrosion-resistant welding wire is greater than 1100 MPa, and the transverse Vickers hardness and the longitudinal Vickers hardness are both greater than 1100 MPa.

[0012] Furthermore, the induction furnace is a vacuum induction furnace.

[0013] Further, the forged square billet is rolled into φ8mm wire rod, pickled, annealed at 1050-1100°C, roughly drawn to φ5mm wire rod, and then subjected to multiple cold drawing, intermediate annealing at 1050-1080°C, and cleaning to obtain φ1.2mm welding wire.

[0014] The beneficial effects of the present invention are:

[0015] The present invention provides a corrosion-resistant welding wire, which can play a role of surface enrichment and protection by adding copper to the nickel-based alloy, and can reduce the stress corrosion sensitivity of the alloy in high-temperature water and gas atmosphere containing chloride ions and cations, so that the welding wire can resist corrosion by high-temperature chloride ions and molten salts, corrosion by high-temperature sulfuric anhydride, oxidation, etc., as well as corrosion by acids and alkalis of different concentrations and corrosion in strong oxidizing environments. Compared with existing nickel-based welding wires, the welding wire has better corrosion resistance, and solves the problem that existing nickel-based welding wires cannot meet the corrosion resistance requirements in high-temperature chloride ion and strong oxidizing acidic environments.

[0016] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. DETAILED DESCRIPTION

[0017] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0018] Example 1

[0019] A corrosion-resistant welding wire consists of the following components in parts by mass: 23%≤Cr≤25%, Fe≤5%, 6%≤Mo≤8%, 3%≤Cu≤4.5%, 3%≤W≤5%, C≤0.1%, Si≤0.5%, Mn≤0.5%, P≤0.02%, S≤0.015%, impurities≤0.5%, and the balance is Ni, with Ni≥51%.

[0020] The method for preparing the corrosion-resistant welding wire comprises the following steps:

[0021] According to the above alloy composition, different types of alloy elements are weighed according to the proportion and mixed, and then melted in an induction furnace (vacuum induction heating melting furnace) to obtain a primary master alloy ingot;

[0022] After electroslag remelting or vacuum self-consumption, a secondary refined master alloy ingot is obtained, which is then forged after being kept at 1000-1080°C for 1-2.5 hours to obtain a forged square billet;

[0023] The forged square billet is rolled into φ8mm wire rod, pickled, annealed at 1050-1100℃, roughly drawn, drawn to 5mm, and then cold drawn multiple times and intermediate annealed at 1050-1080℃ and cleaned to obtain φ1.2mm welding wire. It should be noted that the above-mentioned annealing treatment, rough drawing, continuous cold drawing and intermediate annealing processes are commonly used processes in the prior art, and their specific time parameters can be adaptively adjusted according to the length and size of the wire rod.

[0024] According to the above specific implementation method, a corrosion-resistant welding wire was prepared by smelting, and its chemical composition was analyzed. The results are shown in Table 1.

[0025] Table 1

[0026]

[0027] According to the national standard GB / T 15620-2008 "Nickel and Nickel Alloy Welding Wire", the performance of the above welding wire was tested. The results are shown in Table 2. All indicators of the corrosion-resistant welding wire meet the national standards, and it has good tensile strength and hardness, which can fully meet the comprehensive performance requirements of welding wire under various working environments.

[0028] Table 2

[0029]

[0030] Finally, an intergranular corrosion test was performed on the corrosion-resistant welding wire to detect the corrosion rate of the welding wire. The results are shown in Table 3. The corrosion rate of the corrosion-resistant welding wire is 0.263 mm / year, which is less than the corrosion rate requirement of 0.6 mm / year in the Handbook of Corrosion Date, indicating that the corrosion-resistant welding wire prepared by the present invention has excellent corrosion resistance.

[0031] Table 3

[0032] Sample No. Surface treatment Mass loss (g) Corrosion rate (mm / year) Sample 1 120 grit sandpaper for polishing 0.019 0.263

[0033] In another embodiment, the forged square billet can be rolled into a wire rod of corresponding size, which can be drawn into a wire rod of smaller size through annealing and rough drawing process, and then can be made into welding wire of specified size through continuous cold drawing, intermediate annealing and cleaning.

[0034] Specifically, welding wires of φ1.6mm, φ1.14, φ1.0, φ2.0, φ2.4 etc. can be prepared. The size of the wire rod is adjusted adaptively according to the size of the welding wire.

[0035] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A corrosion-resistant welding wire, characterized in that: It is composed of the following components in parts by mass: 23%≤Cr≤25%, Fe≤5%, 6%≤Mo≤8%, 3%≤Cu≤4.5%, 3%≤W≤5%, C≤0.1%, Si≤0.5%, Mn≤0.5%, P≤0.02%, S≤0.015%, the balance is Ni and ≥51%, and impurities ≤0.5%.

2. A method for preparing a corrosion-resistant welding wire, characterized in that: The following steps are involved: According to the alloy composition of claim 1, different types of alloy elements are weighed according to the proportion, mixed, and then smelted in an induction furnace to obtain a primary master alloy ingot; After electroslag remelting or vacuum self-consumption, a secondary refined master alloy ingot is obtained, which is then forged after being kept at 1000-1080°C for 1-2.5 hours to obtain a forged square billet; The forged square billet is hot rolled into a wire rod of a specified size, and then the welding wire of the specified size is obtained after annealing, rough wire drawing, continuous cold drawing and intermediate annealing.

3. The method for preparing a corrosion-resistant welding wire according to claim 2, characterized in that: The corrosion-resistant welding wire has a tensile strength greater than 1100 MPa, and a transverse Vickers hardness and a longitudinal Vickers hardness both greater than 1100 MPa.

4. The method for preparing a corrosion-resistant welding wire according to claim 2, characterized in that: The induction furnace is a vacuum induction furnace.

5. The method for preparing a corrosion-resistant welding wire according to claim 2, characterized in that: The forged square billet is hot rolled into φ8mm wire rod, which is straightened into φ5mm wire rod by coarse grain wire after annealing treatment, and then φ1.2mm welding wire is obtained after continuous cold drawing and intermediate annealing process.