Self-supporting SAPO-11 molecular sieve as well as preparation method and application thereof
Through the hydrothermal reaction method of phosphorus source, aluminum source, silicon source and imidazole compound, SAPO-11 molecular sieve with a diameter of 2-80 μm was prepared, solving the problems of large grain size and high preparation cost in the prior art, and achieving small Size, low-cost and environmentally friendly catalyst preparation significantly improves the service life of the catalyst.
Patent Information
- Application Number
- CN202310499308.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-05
AI Technical Summary
The existing SAPO-11 molecular sieve has large grain sizes, high preparation costs, and has problems of heterophasic phases and environmental pollution in large-scale industrial production.
Using a hydrothermal reaction method with phosphorus source, aluminum source, silicon source, structural guide R1 and imidazole compounds as additives, a fluffy spherical aggregate SAPO-11 molecular sieve with a diameter of 2-80 μm was formed by aging and crystallization, with an average pore size of 30-55nm, the median pore size is 40-65nm, avoiding ultrasonic or microwave treatment and the use of harmful substances.
The SAPO-11 molecular sieve has a small grain size and low preparation cost, which improves the service life of the catalyst and simplifies the preparation process, which is suitable for industrial large-scale production.
Smart Images

Figure CN118894537A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of molecular sieve synthesis, and in particular to a self-supporting SAPO-11 molecular sieve and a preparation method and application thereof. Background Art
[0002] Molecular sieves are a class of substances with uniform micropores, whose pore size is comparable to that of general molecules. They are widely used in the fields of petrochemicals, agriculture and animal husbandry, environmental protection, and high-tech technologies. Some molecular sieves can be obtained from nature, however, most of the molecular sieves that have been put into practical use in the field of catalysis are obtained through artificial synthesis. Hydrothermal synthesis is the most commonly used method for synthesizing molecular sieves. Some molecular sieves with important industrial applications, such as type A molecular sieves, type X molecular sieves, type Y molecular sieves, ZSM-5 molecular sieves, etc. can be obtained through hydrothermal synthesis. With the advancement of synthesis technology and the diversification of synthesis methods, microwave, supercritical and other technologies have been applied to the synthesis of molecular sieves. SAPO-11 molecular sieve has excellent performance in the skeletal isomerization reaction of carbon chains due to its special pore structure and acidity. Therefore, it has been widely studied.
[0003] US20180264447A1 used ethylene glycol as solvent, filled carbon dioxide into the reactor, and crystallized at 200°C for 144h to obtain small-grain SAPO-11 molecular sieve; the literature (Materials Letters 228(2018)61–64; https: / / doi.org / 10.1016 / j.matlet.2018.05.118) used ultrasonic pretreatment of crystallization liquid, di-n-propylamine as template, and ethanol as solvent to prepare SAPO-11 molecular sieve with special screw morphology; the literature (Fuel 255(2019)115821; https: / / doi.org / 10.1016 / j.fuel.2019.115821) used complex polymers (F127, EO 106 PO 70 EO 106 ) is a mesoporous pore-forming agent, and a multi-level pore SAPO-11 molecular sieve is obtained in a supercritical carbon dioxide system. Patent CN108996518A uses solid acid to post-treat SAPO-11 molecular sieve under different conditions to obtain a SAPO-11 molecular sieve with multi-level pore properties.
[0004] In addition, the research group of RyongRyoo published an article (Nature, 2009, 461 (10): 246-250) reporting for the first time the use of long-chain double-headed quaternary ammonium salts as templates to obtain nanosheet self-supporting MFI crystals for the first time. The diffusion path of the product was shortened during the catalytic reaction, which greatly extended the life span. In the course of the experiment, this research group found that the use of single-headed quaternary ammonium salts with the assistance of imidazole compounds can also obtain self-supporting SAPO-11 molecular sieves. So far, SAPO-11 molecular sieves with this morphology have not been reported.
[0005] In the prior art and research, it can be found that the commonly used templates for synthesizing SAPO-11 are diethylamine, dipropylamine or diisopropylamine, but the crystal size of the synthesized molecular sieve is generally large. In order to reduce the crystal size, expensive surfactants (such as hexadecyltrimethylammonium bromide), HF (aq) and other special additives are usually added, which is not conducive to industrial amplification, and the crystal size (thickness) is still not small enough. Although the microwave method has great advantages in time cost, it is easy to cause crystal transformation during the crystallization process, resulting in impurities, which is not conducive to the preparation of pure phase SAPO-11 molecular sieves. At the same time, the microwave method is not conducive to industrial large-scale production.
[0006] In view of the shortcomings of the prior art, the present invention aims to propose a preparation method that is not involved in the prior art, does not require the addition of additional surfactants, and does not require the use of environmentally harmful substances. The raw materials are cheap and readily available, the operation is simple, the repeatability is good, and it is easy to industrialize and mass produce. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of large size and high preparation cost of the self-supporting SAPO-11 molecular sieve in the prior art, and to provide a self-supporting SAPO-11 molecular sieve and a preparation method and application thereof. The self-supporting SAPO-11 molecular sieve has the characteristics of small size and low preparation cost.
[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a self-supporting SAPO-11 molecular sieve, which is a fluffy spherical aggregate with a diameter of 2-80 μm, and the spherical aggregate is formed by the aggregation of primary thin plate grains with a thickness of 15-50 nm. The average pore size of the molecular sieve is 30-55 nm, and the median pore size is 40-65 nm.
[0009] The second aspect of the present invention provides a method for preparing the molecular sieve of the present invention, the method comprising: preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.2-0.95) R1: (0.3-1.0) R2: (45-110) H2O; the structure directing agent R1 is selected to have a structure as shown in formula (I); the additive R2 is an imidazole compound;
[0010]
[0011] In formula (I), n=5-6; R1, R2, R3, R4, and R5 are each independently selected from a linear alkyl group having 1 to 3 carbon atoms or a linear alkyl group substituted with a hydroxyl group, and may be the same or different.
[0012] The third aspect of the present invention provides an application of the molecular sieve in catalyst preparation.
[0013] Through the above technical solution, the present invention has the following beneficial effects:
[0014] The invention provides a self-supporting SAPO-11 molecular sieve with small grain size. The molecular sieve has a smaller dimension in a certain direction, which is beneficial to the diffusion of small organic molecules and reduces the probability of carbon deposition in the reaction. Therefore, the molecular sieve has a longer service life in the reaction than general grains with the same structure.
[0015] The catalyst of the present invention is prepared by the method of the present invention. The synthesis process does not require ultrasonic or microwave treatment, and does not require the addition of complex organic surfactants and environmentally harmful substances such as HF, so that the preparation process is simple, economical, and environmentally friendly. The raw materials are cheap and easy to obtain, which has great advantages in actual industrial applications.
[0016] The molecular sieve of the present invention is used for catalyst preparation, which can significantly increase the service life of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is the XRD pattern of the molecular sieve of Example 1;
[0018] Figure 2 This is a SEM image of the molecular sieve of Example 1 magnified 20,000 times;
[0019] Figure 3 This is a SEM image of the molecular sieve of Example 1 magnified 2,000 times;
[0020] Figure 4 is the XRD pattern of the molecular sieve of Comparative Example 1;
[0021] Figure 5 This is a SEM image of the molecular sieve of Comparative Example 1 magnified 20,000 times;
[0022] Figure 6 This is the XRD pattern of Comparative Example 2. DETAILED DESCRIPTION
[0023] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0024] The first aspect of the present invention provides a self-supporting SAPO-11 molecular sieve, which is a fluffy spherical aggregate with a diameter of 2-60 μm, and the spherical aggregate is formed by the aggregation of primary thin plate grains with a thickness of 15-50 nm. The average pore size of the molecular sieve is 30-55 nm, and the median pore size is 40-65 nm.
[0025] The present invention provides a self-supporting SAPO-11 molecular sieve with a small grain size. The molecular sieve has a smaller dimension in a certain direction, which is beneficial to the diffusion of small organic molecules and reduces the probability of carbon deposition in the reaction. Therefore, the molecular sieve should have a longer service life in the reaction than general grains with the same structure.
[0026] According to a preferred embodiment of the present invention, the molecular sieve is a fluffy spherical aggregate with a diameter of 2-60 μm, and the spherical aggregate is formed by aggregation of primary thin plate grains with a thickness of 20-50 nm. The average pore size of the molecular sieve is 40-50 nm, and the median pore size is 45-55 nm.
[0027] The second aspect of the present invention provides a method for preparing the molecular sieve of the present invention, the method comprising: preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.2-0.95) R1: (0.3-1.0) R2: (45-110) H2O; the structure directing agent R1 is selected to have a structure as shown in formula (I); the additive R2 is an imidazole compound;
[0028]
[0029] In formula (I), n=5-6; R1, R2, R3, R4, and R5 are each independently selected from a linear alkyl group having 1 to 3 carbon atoms or a linear alkyl group substituted with a hydroxyl group, and may be the same or different.
[0030] The catalyst of the present invention is prepared by the method of the present invention. The synthesis process does not require ultrasonic or microwave treatment, and does not require the addition of complex organic surfactants and environmentally harmful substances such as HF, so that the preparation process is simple, economical, and environmentally friendly. The raw materials are cheap and easy to obtain, which has great advantages in actual industrial applications.
[0031] In the present invention, the silicon source may be a common silicon-containing compound in the art. According to a preferred embodiment of the present invention, the silicon source is selected from at least one of silica sol and fumed silica.
[0032] In the present invention, the aluminum source can be a common aluminum-containing compound in the art. According to a preferred embodiment of the present invention, the aluminum source is selected from at least one of pseudo-boehmite, aluminum isopropoxide, aluminum sulfate, aluminum chloride and aluminum hydroxide.
[0033] In the present invention, the phosphorus source may be a common phosphorus-containing compound in the art. According to a preferred embodiment of the present invention, the phosphorus source is selected from at least one of phosphoric acid, phosphorous acid, ammonium hydrogen phosphate and diammonium phosphate.
[0034] According to a preferred embodiment of the present invention, the method further comprises cooling, separating, washing, drying and calcining the crystallized product.
[0035] According to a preferred embodiment of the present invention, the cooling, separation and washing conditions may be conventionally selected in the art and are not particularly limited in the present invention.
[0036] In the present invention, the drying conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the drying conditions include: a drying temperature of 50-200°C, preferably 80-120°C, and / or a drying time of 5-30h, preferably 8-15h.
[0037] In the present invention, the calcination conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the calcination conditions include: a calcination temperature of 350-700°C, preferably 450-600°C; and / or a calcination time of 1-15h, preferably 5-8h.
[0038] According to a preferred embodiment of the present invention, the crystallized product is cooled, separated and washed before drying. The cooling, separation and washing conditions can be conventionally selected in the art as long as the purpose of the present invention can be achieved.
[0039] In the present invention, the aging conditions may be conventionally selected in the art. According to a preferred embodiment of the present invention, the aging conditions include: an aging temperature of 20-40° C. and an aging time of 2-15 h.
[0040] In the present invention, the crystallization conditions can be conventionally selected in the art. According to a preferred embodiment of the present invention, the crystallization conditions include: a crystallization temperature of 180-210°C, preferably 190-205°C; and / or a crystallization time of 2-24h, preferably 4-18h.
[0041] According to a preferred embodiment of the present invention, the aging and crystallization can be carried out in a crystallization kettle lined with polytetrafluoroethylene, preferably in a dynamic aging and crystallization manner, more preferably in an agitated condition.
[0042] According to a preferred embodiment of the present invention, the molar ratio of each substance in the reaction mixture is: (0.05-0.3) SiO2: (0.8-1.0) Al2O3: 1P2O5: (0.2-0.5) R1: (0.3-0.8) R2: (60-90) H2O,
[0043] According to a preferred embodiment of the present invention, the imidazole compound is selected from at least one of imidazole, 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-butylimidazole, 1-(2-aminoethyl)imidazole and 1-(3-aminopropyl)imidazole.
[0044] According to a preferred embodiment of the present invention, the structure directing agent R1 is selected from at least one of N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide, N,N-dimethylaminohexyl-2-ethyldimethylammonium bromide and hexamethonium.
[0045] In the present invention, the preparation step of the hydrothermal reaction mixture can be a conventional choice in the art. According to a preferred embodiment of the present invention, the preparation step of the hydrothermal reaction mixture is:
[0046] 1) dissolving an aluminum source and a phosphorus source in water to obtain a mixed solution I;
[0047] 2) adding a mixture of the template R1, the additive R2 and water to the mixed solution I to obtain a mixed solution II;
[0048] 3) Adding a silicon source to the mixed solution II to obtain a hydrothermal reaction mixed solution.
[0049] The third aspect of the present invention provides an application of the molecular sieve in catalyst preparation.
[0050] The molecular sieve of the present invention is used for catalyst preparation, which can significantly increase the service life of the catalyst.
[0051] The present invention will be described in detail below by way of examples. In the following examples, the structure of the molecular sieve is determined by an X-ray diffraction spectrum (XRD), and the X-ray diffraction spectrum (XRD) of the molecular sieve is determined by an X-ray powder diffraction (XRD) instrument, using a Cu-Kα ray source, with a Kα1 wavelength λ=1.5405980 angstroms. Nickel filter, working voltage 40kV, current 40mA, scanning range 3-50°. The product morphology was photographed by Japanese emission scanning electron microscope (Fe-SEM); the average pore size and median pore size were determined by mercury intrusion pore size analyzer, and its technical indicators Pascal 140 low-pressure mercury intrusion instrument: pore size: 116~3.8μm, pressure range 0.1~400KPa; Pascal 240 high-pressure mercury intrusion instrument: pore size: 15~0.0074μm, maximum pressure 200MPa.
[0052] Unless otherwise specified, all raw materials were commercially available.
[0053] Example 1
[0054] Weigh 1.9g of pseudo-boehmite (wherein the alumina content is 70wt%, the same below), add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.32g of 1-(3-aminopropyl)imidazole and 3.8g of water, a mixture of 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide and 10g of water to mixed solution I, stir at room temperature for 4h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 7h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. Figure 1 is the XRD pattern of the obtained molecular sieve, which can be seen to be SAPO-11 molecular sieve; Figure 2 (Magnified 20,000 times), Figure 3 (Magnified 2000 times) are SEM images of the molecular sieve obtained by scanning electron microscope at different magnifications. It can be seen that the molecular sieve is a self-supporting fluffy spherical aggregate obtained by the aggregation of primary thin sheet grains. From the high-magnification scanning electron microscope, it can be seen that the thickness of the nanosheet is in the range of 20-50nm, and the diameter of the spherical aggregate is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 41.76nm and the median pore size is 51.28nm.
[0055] Example 2
[0056] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.32g of 1-(3-aminopropyl) imidazole and 3.8g of water, a mixture of 1.8g of 6-N,N-dimethylaminohexyl-dimethyl-propyl ammonium bromide and 10g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 7h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 40.95nm and the median pore size is 53.768nm.
[0057] Example 3
[0058] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.32g of 1-(3-aminopropyl) imidazole and 10g of water, a mixture of 1.5g of 6-N,N-dimethylaminohexyl-dimethyl-ethylammonium bromide and 7.5g of water to mixed solution I, stir at room temperature for 4h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 7h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 41.16nm and the median pore size is 52.17nm.
[0059] Example 4
[0060] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.1g of 1-(3-aminopropyl) imidazole and 3.8g of water, 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyl dimethyl ammonium bromide and 3.8g of water to mixed solution I, stir at room temperature for 5h to obtain mixed solution II; then add 0.23g of 40% silica sol to mixed solution II and stir overnight. Crystallize at 185℃ for 20h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 41.99nm and the median pore size is 53.64nm.
[0061] Example 5
[0062] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.32g of 1-(3-aminopropyl) imidazole and 3.8g of water, a mixture of 1.5g of 5-N,N-dimethylaminohexyl-2-hydroxyethyl dimethyl ammonium bromide and 10g of water to mixed solution I, stir at room temperature for 4h to obtain mixed solution II; then add 0.23g of 40% silica sol to mixed solution II and stir overnight. Crystallize at 205℃ for 5h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 43.39nm and the median pore size is 56.08nm.
[0063] Example 6
[0064] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 0.57g of 1-(3-aminopropyl) imidazole and 3.8g of water, 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyl dimethyl ammonium bromide and 3.8g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 190℃ for 16h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 42.79nm and the median pore size is 53.98nm.
[0065] Example 7
[0066] Weigh 7.2g of aluminum isopropoxide, add 9g of water, stir at room temperature for 2h, fully hydrolyze, then add 3.45g of 85% phosphoric acid, stir at room temperature for 2h, and obtain mixed solution I; then add a mixture of 1.32g of 1-(3-aminopropyl) imidazole and 3.8g of water, a mixture of 1.5g of 5-N,N-dimethylaminopentyl-2-hydroxyethyl dimethyl ammonium bromide and 10g of water to mixed solution I, stir at room temperature for 3h, and obtain mixed solution II; then add 0.36g of nano-silicon dioxide to mixed solution II, and stir overnight. Crystallize at 200℃ for 7h. Cool to room temperature, centrifuge, and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin sheet crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 41.96nm and the median pore size is 52.36nm.
[0067] Example 8
[0068] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 0.93g of imidazole and 3.8g of water, a mixture of 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide and 10g of water to mixed solution I, stir at room temperature for 4h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 8h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 42.66nm and the median pore size is 55.28nm.
[0069] Example 9
[0070] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.5g of 1-propyl imidazole and 3.8g of water, a mixture of 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyl dimethyl ammonium bromide and 10g of water to mixed solution I, stir at room temperature for 3h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 8h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 43.47nm and the median pore size is 54.73nm.
[0071] Example 10
[0072] Weigh 1.9g of pseudo-boehmite, add 9g of water, then add 3.45g of 85% phosphoric acid, stir at room temperature for 3h to obtain mixed solution I; then add a mixture of 1.11g of 1-methylimidazole and 3.8g of water, a mixture of 1.5g of 6-N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide and 10g of water to mixed solution I, stir at room temperature for 5h to obtain mixed solution II; then add 0.09g of nano-silicon dioxide to mixed solution II and stir overnight. Crystallize at 200℃ for 8h. Cool to room temperature, centrifuge and wash. The obtained solid material is dried at 110℃ overnight and calcined at 550℃ for 5h to obtain a molecular sieve. The XRD pattern and SEM pattern of the prepared molecular sieve are the same as those in Example 1. It can be seen that the molecular sieve is SAPO-11 molecular sieve, which is a self-supporting fluffy spherical aggregate obtained by aggregating primary thin plate crystals. From the high-power scanning electron microscope, it can be seen that the thickness of the nanosheets is in the range of 20-50nm, and the diameter of the spherical aggregates is in the range of 20-50μm. The mercury intrusion pore size analyzer measured that the average pore size of the molecular sieve is 44.76nm and the median pore size is 55.46nm.
[0073] Comparative Example 1
[0074] The same as Example 1, except that 1-(3-aminopropyl)imidazole was not added and the ratios of other raw materials remained unchanged to obtain a molecular sieve. Figure 4 is the XRD pattern of the obtained molecular sieve, which can be seen to be SAPO-11 molecular sieve; Figure 5 This is a SEM image of the molecular sieve obtained by scanning electron microscopy with a magnification of 20,000 times. It can be seen that the molecular sieve is a non-spherical aggregate.
[0075] Comparative Example 2
[0076] The same as Example 1, except that 6-N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide is not added, and the ratio of other raw materials remains unchanged to obtain a molecular sieve. Figure 6 : is the XRD pattern of the obtained molecular sieve, it can be seen that the molecular sieve is not SAPO-11 molecular sieve.
[0077] It can be seen from the results of the examples that the molecular sieve of the present invention has a small size and a long service life.
[0078] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A self-supporting SAPO-11 molecular sieve, characterized in that: The molecular sieve is a fluffy spherical aggregate with a diameter of 2-80 μm, which is formed by aggregation of primary thin-plate crystal grains with a thickness of 15-60 nm. The average pore size of the molecular sieve is 30-55 nm, and the median pore size is 40-65 nm.
2. The molecular sieve according to claim 1, wherein The molecular sieve is a fluffy spherical aggregate with a diameter of 2-60 μm, and the spherical aggregate is formed by aggregation of primary thin-plate crystals with a thickness of 20-50 nm. The average pore size of the molecular sieve is 40-50 nm, and the median pore size is 45-55 nm.
3. The method for preparing the molecular sieve according to claim 1 or 2, characterized in that: The method comprises: preparing a hydrothermal reaction mixture with a phosphorus source, an aluminum source, a silicon source, a structure directing agent R1 and an additive R2, aging and crystallizing the reaction mixture, wherein the molar ratio of each substance is: (0.01-0.5) SiO2: (0.8-1.2) Al2O3: 1P2O5: (0.2-0.95) R1: (0.3-1.0) R2: (45-110) H2O; the structure directing agent R1 is selected to have a structure as shown in formula (I); the additive R2 is an imidazole compound; In formula (I), n=5-6; R1, R2, R3, R4, and R5 are each independently selected from a linear alkyl group having 1 to 3 carbon atoms or a linear alkyl group substituted with a hydroxyl group, and may be the same or different.
4. The preparation method according to claim 3, wherein The method further comprises cooling, separating, washing, drying and calcining the crystallized product.
5. The preparation method according to claim 4, wherein: The drying conditions include: a drying temperature of 50-200° C., preferably 80-120° C., and / or a drying time of 5-30 hours, preferably 8-15 hours; and / or The calcination conditions include: a calcination temperature of 350-700° C., preferably 450-600° C.; and / or a calcination time of 1-15 hours, preferably 5-8 hours.
6. The preparation method according to any one of claims 3 to 5, wherein: The aging conditions include: aging temperature of 20-40° C., aging time of 2-15 h; and / or The crystallization conditions include: a crystallization temperature of 180-210° C., preferably 190-205° C.; and / or a crystallization time of 2-24 h, preferably 4-18 h.
7. The preparation method according to any one of claims 3 to 6, wherein: The molar ratio of each substance in the reaction mixture is preferably: (0.05-0.3) SiO2: (0.8-1.0) Al2O3: 1P2O5: (0.2-0.5) R1: (0.3-0.8) R2: (60-90) H2O.
8. The preparation method according to any one of claims 3 to 7, wherein: The imidazole compound is at least one selected from imidazole, 1-methylimidazole, 1-ethylimidazole, 1-propylimidazole, 1-butylimidazole, 1-(2-aminoethyl)imidazole and 1-(3-aminopropyl)imidazole; and / or The structure directing agent R1 is selected from at least one of N,N-dimethylaminohexyl-2-hydroxyethyldimethylammonium bromide, N,N-dimethylaminohexyl-2-ethyldimethylammonium bromide and hexamethonium.
9. The preparation method according to any one of claims 3 to 8, wherein: The preparation steps of the hydrothermal reaction mixture are: 1) dissolving an aluminum source and a phosphorus source in water to obtain a mixed solution I; 2) adding a mixture of the template R1, the additive R2 and water to the mixed solution I to obtain a mixed solution II; 3) Adding a silicon source to the mixed solution II to obtain a hydrothermal reaction mixed solution.
10. Use of the molecular sieve according to claim 1 or 2 in the preparation of catalysts.
Citation Information
Patent Citations
Multi-stage porous SAPO-11 molecular sieve and synthesis method and application thereof
CN108996518A
SAPO-11 Molecular Sieve, Preparation Method thereof, and Use thereof in Hydrocarbon Isomerization
US20180264447A1
Method for synthesizing SAPO-11 molecular sieve by using long chain alkyl silane as silicon source
CN101913621A
Synthesis method and application of small-particle-size SAPO-11 molecular sieve
CN103241745A
SAPO-11 molecular sieve and synthesis method thereof
CN114380299A