Method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum
Alumina is extracted through crushing, grinding and acid leaching, and roasting with phosphogypsum, combined with resin adsorption technology, the problem of low resource utilization of coal gangue and phosphogypsum is solved, and efficient production of silicon fertilizers and industrial raw materials is achieved. , reduce pollution and costs and improve resource utilization.
Patent Information
- Application Number
- CN202410927653.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
The low resource utilization rate of industrial solid waste such as coal gangue and phosphogypsum has led to environmental pollution and waste of resources, and hindered the sustainable development of the coal and phosphochemical industries.
Alumina is extracted through crushing, grinding, acid leaching, and calcining with phosphogypsum to generate silicon fertilizer and sulfuric acid. Combined with resin adsorption technology, high-purity extraction of alumina and ammonium aluminum sulfate is achieved to form high-efficiency silicon fertilizer and industrial raw material.
It has achieved efficient resource utilization of valuable elements in coal gangue and phosphogypsum, and produced high-purity ammonium aluminum sulfate and iron sulfate, which has reduced process costs, reduced pollution, improved resource utilization, and has significant economic and environmental value.
Smart Images

Figure CN118894544A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid waste resource utilization, and in particular to a method for high-silicon coal gangue and phosphogypsum efficient resource comprehensive utilization. Background Art
[0002] Coal gangue is a large amount of industrial solid waste generated during coal mining and processing, and its emissions and stockpiles rank first among industrial solid wastes. The acidic wastewater and heavy metal wastewater produced by long-term weathering and erosion of open-air piled coal gangue will seriously pollute the soil, groundwater and surrounding ecosystems, posing a serious threat to the local ecological environment. For a long time, the resource utilization and harmless treatment of coal gangue have been supported by many policies and regulations, and it is a hot topic of research. Relevant research can be summarized as follows: backfilling of goafs, large-scale treatment such as production of building materials, reclamation and greening, resource recovery, etc. Although great progress has been made, its comprehensive utilization rate is still less than 30%. Coal gangue contains a large amount of Al 2 O 3 and SiO 2 Resources, in addition, it also contains varying amounts of metals such as Fe, Ti, V, Co and Ga. With the expansion and deepening of research and the gradual improvement of environmental protection requirements, coal gangue has also been regarded as a "misplaced raw material" in recent years. Relevant workers have conducted a lot of research on its resource utilization. The resource utilization of this type of solid waste can completely eliminate the harm it causes and is conducive to economic development. It is an important and scientifically reasonable idea.
[0003] Phosphogypsum is a solid waste generated in the wet phosphoric acid process, and its main component is calcium sulfate dihydrate. The composition of phosphogypsum is relatively complex. In addition to calcium sulfate, there are also incompletely decomposed phosphate ore, residual phosphoric acid, fluoride, acid insoluble matter, organic matter, etc. Among them, the presence of fluorine and organic matter has the greatest impact on the resource utilization of phosphogypsum. The random discharge and accumulation of phosphogypsum has seriously damaged the ecological environment, not only polluting groundwater resources, but also causing waste of land resources. The "Action Plan for the Prevention and Control of Soil Pollution" has put forward strict requirements for soil governance. It clearly points out that the treatment of industrial waste such as phosphogypsum should be increased. The random accumulation and discharge of phosphogypsum has restricted the sustainable development of wet phosphoric acid, phosphate fertilizer and other industries, so the treatment and recycling of phosphogypsum has become an imminent issue.
[0004] Silicon fertilizer has been confirmed by the international soil science community as the fourth growth element fertilizer after nitrogen, phosphorus and potassium fertilizers. As a new type of fertilizer, silicon fertilizer plays an increasingly important role in agricultural production. Silicon is an essential growth element for crops. It has the effect of increasing production and improving quality. It is a health fertilizer, quality fertilizer, and nutrition regulating fertilizer. Silicon fertilizer has the effects of anti-lodging, anti-pest and disease resistance, drought resistance, and anti-repeat. Silicon fertilizer has the effects of promoting photosynthesis, promoting root growth and development, and promoting the effective utilization of nutrients. Silicon fertilizer can also effectively passivate heavy metals, reduce heavy metal pollution in the soil, increase soil base, and improve the soil environment. Through replacement reactions, toxic and harmful ions such as iron and aluminum accumulated in the soil are converted into non-toxic substances, reducing the adverse effects of toxic elements in the soil on crops. my country's silicon fertilizer market has great potential.
[0005] In summary, it is of great significance to develop a new method for the efficient resource utilization of high-silicon coal gangue and phosphogypsum, and to utilize the main components of aluminum, silicon and iron in the two industrial solid wastes, coal gangue and phosphogypsum, to ultimately form final products such as silicon fertilizer. Summary of the invention
[0006] The purpose of the present invention is to provide a method for the efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum to solve the existing
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The present invention provides a method for high-silicon coal gangue and phosphogypsum efficient resource comprehensive utilization, comprising the following steps:
[0009] (1) crushing and grinding the gangue in sequence to obtain a gangue grinding product;
[0010] (2) leaching the coal gangue grinding product obtained in step (1) by acid leaching to remove aluminum oxide in the coal gangue grinding product, and obtaining aluminum sulfate solution and acid leaching residue by filtering after the acid leaching reaction is completed;
[0011] (3) mixing the acid leaching residue obtained in step (2) with phosphogypsum and then calcining and modifying the mixture to obtain silicon fertilizer and sulfur dioxide gas;
[0012] (4) the sulfur dioxide gas generated in the roasting process of step (3) is fed into an acid production system to produce sulfuric acid, and the obtained sulfuric acid is returned to the acid leaching process of step (2) as needed;
[0013] (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to react to generate an ammonium aluminum sulfate solution;
[0014] (6) crystallizing the ammonium aluminum sulfate solution obtained in step (5), and performing solid-liquid separation after the crystallization to obtain ammonium aluminum sulfate crystals and mother liquor;
[0015] (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in water, and then subjecting them to recrystallization. After the recrystallization is completed, solid-liquid separation is performed to obtain high-purity ammonium aluminum sulfate and recrystallization mother liquor;
[0016] (8) returning the recrystallization mother liquor obtained in step (7) to the acid leaching process of step (2);
[0017] (9) dissolving the high-purity ammonium aluminum sulfate obtained in step (7) in water again, and then further purifying it by resin adsorption to finally obtain higher-purity ammonium aluminum sulfate;
[0018] (10) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid and crystallized to remove salts therein. After the crystallization is completed, solid-liquid separation is performed to obtain new acid and ferrous sulfate, and the new acid is returned to the acid leaching process of step (2).
[0019] Preferably, in step (1), the grinding includes open-circuit crushing grinding or closed-circuit crushing grinding; and the -0.074 mm particle size accounts for 50 to 90% of the coal gangue grinding product.
[0020] Preferably, in the step (2), the reagent used for acid leaching is sulfuric acid; the acid leaching includes atmospheric pressure acid leaching or pressurized acid leaching; the process parameters of atmospheric pressure acid leaching are as follows: the mass fraction of sulfuric acid is 50-90%, the temperature is 80-170°C, the liquid-to-solid ratio is 1-6:1, and the time is 0.5-3h; the process parameters of pressurized acid leaching are as follows: the mass fraction of sulfuric acid is 10-60%, the temperature is 100-180°C, the liquid-to-solid ratio is 1-6:1, the pressure is 0.1-0.3MPa, and the time is 0.5-3h.
[0021] Preferably, in the step (3), the mass ratio of the acid leaching residue to the phosphogypsum is 1:0.1-10; the temperature for roasting and modification is 600-1100°C, and the time for roasting and modification is 0.5-3h.
[0022] Preferably, in step (5), the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is 1:1-2; the reaction temperature is 80-120°C, and the reaction time is 0.2-3h.
[0023] Preferably, in step (6), the crystallization includes vacuum crystallization or normal pressure crystallization; the process conditions of vacuum crystallization are as follows: vacuum degree is 2000-8000Pa, time is 0.5-2h, and crystallization end temperature is 25-50°C; the process conditions of normal pressure crystallization are as follows: time is 0.5-2h, and crystallization end temperature is 15-50°C.
[0024] Preferably, in step (7), the number of recrystallizations is 0 to 5 times; and the purity of the high-purity ammonium aluminum sulfate is 99 to 99.99%.
[0025] Preferably, in step (9), the number of times of resin adsorption is 0 to 3 times; the purity of the higher purity ammonium aluminum sulfate is 99 to 99.999%.
[0026] Preferably, the solid-liquid separation in step (6), step (7) and step (10) independently comprises filtration or centrifugal separation.
[0027] Preferably, in step (10), the mass fraction of concentrated sulfuric acid is 97-99%; and the volume ratio of mother liquor to concentrated sulfuric acid is 1:0.3-3.
[0028] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. Realize efficient resource utilization and high value of various valuable elements in coal gangue and phosphogypsum at the same time:
[0030] (1) Alumina in coal gangue is finally converted into high-purity ammonium aluminum sulfate through acid leaching, crystallization, recrystallization and resin adsorption. High-purity ammonium aluminum sulfate can be used directly as a product and is also a widely used industrial raw material. It can also be used as an intermediate for the production of metallic aluminum.
[0031] (2) After the extraction of alumina, the silicon oxide in the gangue is modified with phosphogypsum to convert the silicon oxide in the gangue, silicon and calcium in the phosphogypsum into effective silicon and effective calcium that can be absorbed and utilized by plants, producing silicon fertilizer or silicon-calcium fertilizer that is beneficial to plant growth. The sulfur dioxide gas produced during the roasting process is recycled for the preparation of sulfuric acid, and the prepared sulfuric acid can be returned to the acid leaching process of the gangue as a leaching agent, thereby achieving efficient utilization of resources and reducing the cost of reagents in the process;
[0032] (3) Resource utilization: The iron in the coal gangue is recovered and an iron sulfate product is produced. The iron sulfate can be used to produce sulfuric acid. In the current production of power batteries for new energy vehicles, iron sulfate is an important raw material for producing lithium-ion batteries. The present invention realizes the high value of this part of resources.
[0033] 2. The present invention can generate important economic and environmental values:
[0034] The present invention fully utilizes coal gangue and phosphogypsum at the same time, and no new secondary pollutants are generated in the process. The large-scale storage of coal gangue and phosphogypsum restricts the development of their respective coal industry and phosphorus chemical industry. The increasingly severe environmental protection problems pose a threat to the surrounding ecological environment and human health. The present invention utilizes and increases the value of originally worthless solid waste, and generates better economic benefits in the process of turning waste into treasure. The present invention has significant environmental value and economic value, and is in line with the industry's concept of green and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0036] Figure 1 The present invention is a flowchart of the method. DETAILED DESCRIPTION
[0037] The present invention provides a method for high-silicon coal gangue and phosphogypsum efficient resource comprehensive utilization, comprising the following steps:
[0038] (1) crushing and grinding the gangue in sequence to obtain a gangue grinding product;
[0039] (2) leaching the coal gangue grinding product obtained in step (1) by acid leaching to remove aluminum oxide in the coal gangue grinding product, and obtaining aluminum sulfate solution and acid leaching residue by filtering after the acid leaching reaction is completed;
[0040] (3) mixing the acid leaching residue obtained in step (2) with phosphogypsum and then calcining and modifying the mixture to obtain silicon fertilizer and sulfur dioxide gas;
[0041] (4) the sulfur dioxide gas generated in the roasting process of step (3) is fed into an acid production system to produce sulfuric acid, and the obtained sulfuric acid is returned to the acid leaching process of step (2) as needed;
[0042] (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to react to generate an ammonium aluminum sulfate solution;
[0043] (6) crystallizing the ammonium aluminum sulfate solution obtained in step (5), and performing solid-liquid separation after the crystallization to obtain ammonium aluminum sulfate crystals and mother liquor;
[0044] (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in water, and then subjecting them to recrystallization. After the recrystallization is completed, solid-liquid separation is performed to obtain high-purity ammonium aluminum sulfate and recrystallization mother liquor;
[0045] (8) returning the recrystallization mother liquor obtained in step (7) to the acid leaching process of step (2);
[0046] (9) dissolving the high-purity ammonium aluminum sulfate obtained in step (7) in water again, and then further purifying it by resin adsorption to finally obtain higher-purity ammonium aluminum sulfate;
[0047] (10) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid and crystallized to remove salts therein. After the crystallization is completed, solid-liquid separation is performed to obtain new acid and ferrous sulfate, and the new acid is returned to the acid leaching process of step (2).
[0048] In step (1) of the present invention, grinding includes open-circuit crushing grinding or closed-circuit crushing grinding; the proportion of the particle size of ≤0.074 mm in the gangue grinding product is preferably 50-90%, more preferably 60-80%, and more preferably 65-70%. The particle size of the gangue grinding product can ensure the smooth progress of subsequent acid leaching.
[0049] In step (2) of the present invention, the reagent used for acid leaching is sulfuric acid; the acid leaching includes normal pressure acid leaching or pressure acid leaching;
[0050] The process parameters of atmospheric pressure acid leaching are as follows: the mass fraction of sulfuric acid is preferably 50-90%, more preferably 60-80%, more preferably 70-75%; the temperature is preferably 80-170°C, more preferably 90-150°C, more preferably 100-120°C; the liquid-to-solid ratio is preferably 1-6:1, more preferably 2-5:1, more preferably 3-4:1; the time is preferably 0.5-3h, more preferably 1-2.5h, more preferably 1.5-2h;
[0051] The process parameters of pressurized acid leaching are as follows: the mass fraction of sulfuric acid is preferably 10-60%, more preferably 20-50%, and more preferably 30-40%; the temperature is preferably 100-180°C, more preferably 120-160°C, and more preferably 130-150°C; the liquid-to-solid ratio is preferably 1-6:1, more preferably 2-5:1, and more preferably 3-4:1; the pressure is preferably 0.1-0.3MPa, and more preferably 0.2MPa; the time is preferably 0.5-3h, more preferably 1-2.5h, and more preferably 1.5-2h;
[0052] The ultimate goal of regulating the acid leaching conditions is to efficiently leach alumina from the coal gangue grinding products.
[0053] In step (3) of the present invention, the mass ratio of acid leaching residue to phosphogypsum is preferably 1:0.1-10, more preferably 1:2-8, and more preferably 1:5-6; the temperature for roasting modification is preferably 600-1100°C, more preferably 700-1000°C, and more preferably 800-900°C; the time for roasting modification is preferably 0.5-3h, more preferably 1-2.5h, and more preferably 1.5-2h.
[0054] In step (5) of the present invention, the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is preferably 1:1-2, more preferably 1:1.2-1.8, more preferably 1:1.5-1.6; the reaction temperature is preferably 80-120°C, more preferably 95-110°C, more preferably 100-105°C; the reaction time is preferably 0.2-3h, more preferably 0.5-2.5h, more preferably 1-2h.
[0055] In step (6) of the present invention, the crystallization includes vacuum crystallization or normal pressure crystallization;
[0056] The process conditions of vacuum crystallization are as follows: the vacuum degree is preferably 2000-8000Pa, more preferably 3000-6000Pa, more preferably 4000-5000Pa; the time is preferably 0.5-2h, more preferably 1-1.5h; the crystallization end point temperature is preferably 25-50°C, more preferably 30-45°C, more preferably 35-40°C;
[0057] The process conditions of normal pressure crystallization are as follows: the time is preferably 0.5 to 2 hours, more preferably 1 to 1.5 hours; the crystallization end point temperature is preferably 15 to 50°C, more preferably 20 to 45°C, and more preferably 30 to 40°C.
[0058] In step (7) of the present invention, the number of recrystallizations is preferably 0 to 5 times, more preferably 1 to 4 times, and more preferably 2 to 3 times. The number of recrystallizations can be determined according to the purity requirements; the purity of high-purity ammonium aluminum sulfate is 99 to 99.99%.
[0059] In step (9) of the present invention, the number of times of resin adsorption is preferably 0 to 3 times, more preferably 1 to 2 times, and the number of times of resin adsorption can be determined according to the purity requirement; the purity of higher purity ammonium aluminum sulfate is 99 to 99.999%.
[0060] In the present invention, the solid-liquid separation in step (6), step (7) and step (10) independently includes filtration or centrifugal separation.
[0061] In step (10) of the present invention, the mass fraction of concentrated sulfuric acid is preferably 97-99%, more preferably 97.5-98.5%, and more preferably 98%; the volume ratio of mother liquor to concentrated sulfuric acid is preferably 1:0.3-3, more preferably 1:0.5-2, and more preferably 1:1-1.5.
[0062] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0063] Example 1
[0064] This embodiment provides a method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum, comprising the following steps:
[0065] (1) Low-quality high-silicon coal gangue sampled from a coal gangue enterprise in Qujing, Yunnan, has the following chemical composition and content: SiO 2 The content is 48.57%, Al 2 O 3 The content is 19.23%, Fe 2 O 3 The content of SO is 12.01%, the content of CaO is 3.38%, and the content of MgO is 2.78%. The chemical composition and content of phosphogypsum sampled from a phosphate mine in Kunming, Yunnan are as follows: the content of CaO is 31.07%, the content of SO 2 The content is 45.32%, SiO 2 The content is 10.06%, P 2 O 5 The content of is 1.32%, the content of MgO is 0.11%, and the content of Al 2 O 3 The content is 0.12%, Fe 2 O 3 The content is 0.03%;
[0066] The gangue is dried, crushed and ground to form a gangue grinding product with a particle size of -0.074 mm accounting for 80%; the phosphogypsum is dried to prepare a sample for subsequent steps;
[0067] (2) subjecting the gangue grinding product obtained in step (1) to acid leaching, wherein the acid leaching is selected as atmospheric pressure sulfuric acid leaching, and the acid leaching reaction conditions are: the mass fraction of sulfuric acid is 60%, the acid leaching temperature is 150° C., the liquid-solid ratio is 4:1, and the acid leaching time is 2 h. Alumina is extracted by acid leaching, and the leaching rate of alumina in the gangue grinding product reaches 98.96%. After filtering, an aluminum sulfate solution and acid leaching residue are obtained;
[0068] (3) The acid leaching residue obtained in step (2) and phosphogypsum are mixed in a mass ratio of 1:5 and roasted and modified to prepare silicon fertilizer, and sulfur dioxide gas is obtained. The roasting and modification temperature is 1000° C. and the roasting and modification time is 1 h. The technical indicators of the obtained silicon fertilizer are shown in Table 1. The content of effective silicon in the obtained silicon fertilizer is 29.5%, the content of effective calcium is 32.7%, and the contents of other heavy metals and harmful metal elements are lower than the national standard values. The product technical indicators of the obtained silicon fertilizer are high-quality silicon fertilizer, which also contains a large amount of effective calcium, so it can also be regarded as a high-quality silicon-calcium fertilizer;
[0069] Table 1 Technical indicators of silicon fertilizer obtained
[0070] project Test results National standards and marked value requirements Single judgment <![CDATA[Available silicon (SiO 2 ) content / %]]> 29.5 ≥20.0 qualified Moisture content / % 1.8 ≤3.0 qualified Effective calcium (CaO) content / % 32.7 ≥30.0 qualified Mass fraction of arsenic (As) / % Not detected ≤0.0050 qualified Mass fraction of cadmium (Cd) / % 0.00001 ≤0.0010 qualified Mass fraction of lead (Pb) / % 0.0003 ≤0.0200 qualified Mass fraction of mercury (Hg) / % Not detected ≤0.0500 qualified Mass fraction of chromium (Cr) / % 0.0002 ≤0.0005 qualified
[0071] (4) the sulfur dioxide gas generated in the roasting and modification process of step (3) is fed into an acid production system to prepare sulfuric acid, and the prepared sulfuric acid can be returned to the acid leaching process of step (1);
[0072] (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to carry out an ammonium-aluminum reaction at 100° C., and the reaction time is controlled to be 0.5 h to generate an ammonium aluminum sulfate solution, wherein the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is 1:2;
[0073] (6) subjecting the ammonium aluminum sulfate solution obtained in step (5) to vacuum crystallization, wherein the vacuum degree is controlled to be 6000 Pa, the vacuum crystallization time is 0.5 h, the vacuum crystallization end point temperature is 40° C., and after the vacuum crystallization is completed, solid-liquid separation is performed by filtration to obtain ammonium aluminum sulfate crystals and mother liquor;
[0074] (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in deionized water and subjecting them to recrystallization once, wherein the operating conditions of the recrystallization are as follows: the vacuum degree is controlled at 6000 Pa, the recrystallization time is 0.5 h, the recrystallization end point temperature is 40° C., and after the recrystallization is completed, solid-liquid separation is performed by filtration to obtain a recrystallization mother liquor and high-purity ammonium aluminum sulfate with a purity of 99.1%; the recrystallization mother liquor is returned to the acid leaching process of step (1);
[0075] (8) dissolving the high-purity ammonium aluminum sulfate obtained by crystallization in step (7) in deionized water again, and then further purifying it by resin adsorption once, and finally obtaining ammonium aluminum sulfate with a purity of 99.92%, which is recycled;
[0076] (9) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid having a mass fraction of 98% in a volume ratio of 1:1 and allowed to settle. After filtering, ferric sulfate and new acid (sulfuric acid) are obtained. The ferric sulfate is recycled and the new acid (sulfuric acid) is returned to the acid leaching process of step (1).
[0077] Example 2
[0078] This embodiment provides a method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum, comprising the following steps:
[0079] (1) Low-quality high-silicon coal gangue sampled from a coal gangue enterprise in Guizhou, its chemical composition and content are: SiO 2 The content is 42.34%, Al 2 O 3 The content is 15.21%, Fe 2 O 3The content of SO is 15.78%, the content of CaO is 4.01%, and the content of MgO is 1.36%. The chemical composition and content of phosphogypsum sampled from a phosphate mine in Kunming, Yunnan are as follows: the content of CaO is 31.07%, the content of SO 2 The content is 45.32%, SiO 2 The content is 10.06%, P 2 O 5 The content of MgO is 1.32%, the content of Al is 0.14%, 2 O 3 The content is 0.13%, Fe 2 O 3 The content is 0.05%;
[0080] The gangue is dried, crushed and ground to form a gangue grinding product with a particle size of -0.074 mm accounting for 80%; the phosphogypsum is dried to prepare a sample for subsequent steps;
[0081] (2) subjecting the gangue grinding product obtained in step (1) to acid leaching, wherein the acid leaching is selected as atmospheric pressure sulfuric acid leaching, and the acid leaching reaction conditions are: the mass fraction of sulfuric acid is 60%, the acid leaching temperature is 150° C., the liquid-solid ratio is 4:1, and the acid leaching time is 2 h. Alumina is extracted by acid leaching, and the leaching rate of alumina in the gangue grinding product reaches 97.53%. After filtering, an aluminum sulfate solution and an acid leaching residue are obtained;
[0082] (3) The acid leaching residue obtained in step (2) and phosphogypsum are mixed in a mass ratio of 1:8 and roasted to prepare silicon fertilizer, and sulfur dioxide gas is obtained. The roasting modification temperature is 900° C. and the roasting modification time is 2 h. The technical indicators of the obtained silicon fertilizer are shown in Table 2. The content of effective silicon in the obtained silicon fertilizer is 25.4%, the content of effective calcium is 30.6%, and the contents of other heavy metals and harmful metal elements are lower than the national standard values. The product technical indicators of the obtained silicon fertilizer are high-quality silicon fertilizer, which also contains a large amount of effective calcium, so it can also be regarded as a high-quality silicon-calcium fertilizer;
[0083] Table 2 Technical indicators of silicon fertilizer obtained
[0084] project Test results National standards and marked value requirements Single judgment <![CDATA[Effective silicon (SiO 2 ) content / %]]> 25.4 ≥20.0 qualified Moisture content / % 1.8 ≤3.0 qualified Effective calcium (CaO) content / % 30.6 ≥30.0 qualified Mass fraction of arsenic (As) / % Not detected ≤0.0050 qualified Mass fraction of cadmium (Cd) / % 0.00001 ≤0.0010 qualified Mass fraction of lead (Pb) / % 0.0005 ≤0.0200 qualified Mass fraction of mercury (Hg) / % Not detected ≤0.0500 qualified Mass fraction of chromium (Cr) / % 0.0003 ≤0.0005 qualified
[0085] (4) the sulfur dioxide gas generated in the roasting and modification process of step (3) is fed into an acid production system to prepare sulfuric acid, and the prepared sulfuric acid can be returned to the acid leaching process of step (1);
[0086] (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to carry out an ammonium-aluminum reaction at 95° C., and the reaction time is controlled to be 0.5 h to generate an ammonium aluminum sulfate solution, wherein the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is 1:2;
[0087] (6) subjecting the ammonium aluminum sulfate solution obtained in step (5) to normal pressure crystallization, wherein the normal pressure crystallization time is 1 hour, the normal pressure crystallization endpoint temperature is 20° C., and the crystallization rate reaches 95%. After the normal pressure crystallization is completed, solid-liquid separation is performed by filtration to obtain ammonium aluminum sulfate crystals and mother liquor;
[0088] (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in deionized water and subjecting them to two recrystallizations. The operating conditions of the two recrystallizations are the same, and the parameters are as follows: the recrystallization time is 1 hour, the recrystallization end temperature is 20° C., and after the recrystallization is completed, solid-liquid separation is performed by filtering to obtain a recrystallization mother liquor and high-purity ammonium aluminum sulfate with a purity of 99.9%; the recrystallization mother liquor is returned to the acid leaching process of step (1);
[0089] (8) dissolving the high-purity ammonium aluminum sulfate obtained by crystallization in step (7) in deionized water again, and then further purifying it by resin adsorption once, and finally obtaining ammonium aluminum sulfate with a purity of 99.99%, which is recycled;
[0090] (9) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid having a mass fraction of 98% in a volume ratio of 1:1.5 and allowed to settle. After filtering, ferric sulfate and new acid (sulfuric acid) are obtained. The ferric sulfate is recycled and the new acid (sulfuric acid) is returned to the acid leaching process of step (1).
[0091] Example 3
[0092] This embodiment provides a method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum, comprising the following steps:
[0093] (1) Low-quality high-silicon coal gangue sampled from a coal gangue enterprise in Guizhou, its chemical composition and content are: SiO 2 The content is 42.34%, Al 2 O 3 The content is 15.21%, Fe 2 O 3 The content of phosphogypsum is 15.78%, the content of CaO is 4.01%, and the content of MgO is 1.36%. The chemical composition and content of phosphogypsum sampled from a phosphate mine in Guizhou are as follows: the content of CaO is 33.52%, the content of SO 2 The content is 43.21%, SiO 2 The content is 8.69%, P 2 O 5 The content of is 2.08%, the content of MgO is 0.10%, and the content of Al 2 O 3 The content is 0.15%, Fe 2 O 3 The content is 0.03%;
[0094] The gangue is dried, crushed and ground to form a gangue grinding product with a particle size of -0.074 mm accounting for 70%; the phosphogypsum is dried to prepare a sample for subsequent steps;
[0095] (2) subjecting the gangue grinding product obtained in step (1) to acid leaching, wherein the acid leaching is selected as atmospheric pressure sulfuric acid leaching, and the acid leaching reaction conditions are: the mass fraction of sulfuric acid is 50%, the acid leaching temperature is 140° C., the liquid-solid ratio is 4:1, and the acid leaching time is 2 h. Alumina is extracted by acid leaching, and the leaching rate of alumina in the gangue grinding product reaches 98.36%. After filtering, an aluminum sulfate solution and an acid leaching residue are obtained;
[0096] (3) The acid leaching residue obtained in step (2) and phosphogypsum are mixed in a mass ratio of 1:6 and roasted and modified to prepare silicon fertilizer, and sulfur dioxide gas is obtained. The roasting and modification temperature is 1000° C. and the roasting and modification time is 1 h. The technical indicators of the obtained silicon fertilizer are shown in Table 3. The content of effective silicon in the obtained silicon fertilizer is 27.8%, the content of effective calcium is 33.5%, and the contents of other heavy metals and harmful metal elements are all lower than the national standard values. The product technical indicators of the obtained silicon fertilizer are high-quality silicon fertilizer, which also contains a large amount of effective calcium, so it can also be regarded as a high-quality silicon-calcium fertilizer;
[0097] Table 3 Technical indicators of silicon fertilizer obtained
[0098]
[0099]
[0100] (4) the sulfur dioxide gas generated in the roasting and modification process of step (3) is fed into an acid production system to prepare sulfuric acid, and the prepared sulfuric acid can be returned to the acid leaching process of step (1);
[0101] (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to carry out an ammonium-aluminum reaction at 95° C., and the reaction time is controlled to be 0.5 h to generate an ammonium aluminum sulfate solution, wherein the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is 1:1.5;
[0102] (6) subjecting the ammonium aluminum sulfate solution obtained in step (5) to vacuum crystallization, wherein the vacuum degree is controlled to 7000 Pa, the vacuum crystallization time is 0.5 h, the vacuum crystallization end point temperature is 40° C., and after the vacuum crystallization is completed, solid-liquid separation is performed by filtration to obtain ammonium aluminum sulfate crystals and mother liquor;
[0103] (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in deionized water and performing recrystallization twice. The operating conditions of the two recrystallizations are the same, and the parameters are as follows: the vacuum degree is controlled at 7000 Pa, the recrystallization time is 0.5 h, and the recrystallization end temperature is 40° C. After the recrystallization is completed, solid-liquid separation is performed by filtering to obtain a recrystallization mother liquor and high-purity ammonium aluminum sulfate with a purity of 99.9%; the recrystallization mother liquor is returned to the acid leaching process of step (1);
[0104] (8) dissolving the high-purity ammonium aluminum sulfate obtained by crystallization in step (7) in deionized water again, and then further purifying it by resin adsorption once, and finally obtaining ammonium aluminum sulfate with a purity of 99.99%, which is recycled;
[0105] (9) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid having a mass fraction of 98% in a volume ratio of 1:1 and allowed to settle. After filtering, ferric sulfate and new acid (sulfuric acid) are obtained. The ferric sulfate is recycled and the new acid (sulfuric acid) is returned to the acid leaching process of the coal gangue in step (1).
[0106] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum, It is characterized in that The steps include: (1) crushing and grinding the gangue in sequence to obtain a gangue grinding product; (2) leaching the coal gangue grinding product obtained in step (1) by acid leaching to remove aluminum oxide in the coal gangue grinding product, and obtaining aluminum sulfate solution and acid leaching residue by filtering after the acid leaching reaction is completed; (3) mixing the acid leaching residue obtained in step (2) with phosphogypsum and then calcining and modifying the mixture to obtain silicon fertilizer and sulfur dioxide gas; (4) the sulfur dioxide gas generated in the roasting process of step (3) is fed into an acid production system to produce sulfuric acid, and the obtained sulfuric acid is returned to the acid leaching process of step (2) as needed; (5) adding ammonium sulfate to the aluminum sulfate solution obtained in step (2) to react to generate an ammonium aluminum sulfate solution; (6) crystallizing the ammonium aluminum sulfate solution obtained in step (5), and performing solid-liquid separation after the crystallization to obtain ammonium aluminum sulfate crystals and mother liquor; (7) dissolving the ammonium aluminum sulfate crystals obtained in step (6) in water, and then subjecting them to recrystallization. After the recrystallization is completed, solid-liquid separation is performed to obtain high-purity ammonium aluminum sulfate and recrystallization mother liquor; (8) returning the recrystallization mother liquor obtained in step (7) to the acid leaching process of step (2); (9) dissolving the high-purity ammonium aluminum sulfate obtained in step (7) in water again, and then further purifying it by resin adsorption to finally obtain higher-purity ammonium aluminum sulfate; (10) The mother liquor obtained in step (6) is mixed with concentrated sulfuric acid and crystallized to remove salts therein. After the crystallization is completed, solid-liquid separation is performed to obtain new acid and ferrous sulfate, and the new acid is returned to the acid leaching process of step (2).
2. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 1, It is characterized in that In the step (1), the grinding includes open-circuit crushing grinding or closed-circuit crushing grinding; the -0.074 mm particle size accounts for 50 to 90% of the coal gangue grinding product.
3. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 2, It is characterized in that In the step (2), the reagent used for acid leaching is sulfuric acid; the acid leaching includes normal pressure acid leaching or pressurized acid leaching; the process parameters of normal pressure acid leaching are as follows: the mass fraction of sulfuric acid is 50-90%, the temperature is 80-170°C, the liquid-to-solid ratio is 1-6:1, and the time is 0.5-3h; the process parameters of pressurized acid leaching are as follows: the mass fraction of sulfuric acid is 10-60%, the temperature is 100-180°C, the liquid-to-solid ratio is 1-6:1, the pressure is 0.1-0.3MPa, and the time is 0.5-3h.
4. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to any one of claims 1 to 3, It is characterized in that In the step (3), the mass ratio of the acid leaching residue to the phosphogypsum is 1:0.1-10; the roasting and modification temperature is 600-1100°C, and the roasting and modification time is 0.5-3h.
5. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 4, It is characterized in that In the step (5), the molar ratio of aluminum ions in the aluminum sulfate solution to ammonium ions in the ammonium sulfate is 1:1-2; the reaction temperature is 80-120° C., and the reaction time is 0.2-3 h.
6. The method for efficient resource comprehensive utilization of high-silicon coal gangue in collaboration with phosphogypsum according to claim 1, 2, 3 or 5, It is characterized in that In the step (6), the crystallization includes vacuum crystallization or normal pressure crystallization; the process conditions of vacuum crystallization are as follows: vacuum degree is 2000-8000Pa, time is 0.5-2h, and crystallization end temperature is 25-50°C; the process conditions of normal pressure crystallization are as follows: time is 0.5-2h, and crystallization end temperature is 15-50°C.
7. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 6, It is characterized in that In the step (7), the number of recrystallizations is 0 to 5 times; the purity of the high-purity ammonium aluminum sulfate is 99 to 99.99%.
8. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 7, It is characterized in that In the step (9), the number of times of resin adsorption is 0 to 3 times; the purity of the higher purity ammonium aluminum sulfate is 99 to 99.999%.
9. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 7 or 8, It is characterized in that The solid-liquid separation in step (6), step (7) and step (10) independently includes filtration or centrifugal separation.
10. The method for efficient resource comprehensive utilization of high-silicon coal gangue and phosphogypsum according to claim 9, It is characterized in that In the step (10), the mass fraction of concentrated sulfuric acid is 97-99%; and the volume ratio of mother liquor to concentrated sulfuric acid is 1:0.3-3.