Method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium middlings

Through the chlorination leaching method of titanium medium ore, the problem of low utilization rate of titanium medium ore resources is solved, the low cost and environmentally friendly production of titanium dioxide is achieved, the application field is expanded, and the problem of insufficient supply in the titanium concentrate market is solved.

CN118894552AActive Publication Date: 2024-11-05PANZHIHUA ANTAI TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411289411.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-05
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively use titanium medium ore resources to produce nanotitanium dioxide and rutile titanium dioxide, resulting in high production costs and high environmental pressures, and insufficient supply of titanium concentrate market.

Method used

The chlorination leaching method of titanium medium ore is used to preactivate titanium medium ore fine material by grinding and microwave preactivated, combined with hydrochloric acid analysis system, and the chlorinated slurry is produced, and nanometers are prepared by thermal filtration, freezing crystallization, spray roasting and other steps. Titanium dioxide and rutile titanium dioxide achieve efficient utilization of titanium resources.

Benefits of technology

It improves the resource utilization rate of titanium in vanadium titanium magnetite, reduces production costs, realizes environmentally friendly industrial production, expands the application field of by-products, and avoids environmental pollution in ore dressing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894552A_ABST
    Figure CN118894552A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium middlings. The method comprises the following steps: (1) grinding and microwave pre-activating a titanium middling raw material; (2) chlorination leaching; (3) filtering to obtain fine filtering leachate; (4) freezing and crystallizing the finely filtered leaching solution to obtain a clear titanium solution; (5) the clear titanium solution is divided into two parts, one part is used for preparing nanometer titanium dioxide, and the other part is used for preparing rutile titanium dioxide; according to the method, comprehensive utilization of the vanadium titano-magnetite is achieved, the nano titanium dioxide and rutile titanium dioxide which are high in added value and are comprehensively prepared through chlorination leaching of the titanium middlings are developed, the production cost is low, hydrochloric acid is recycled, and the production process is environmentally friendly. According to the method, the titanium middlings can be used as the raw material, and the grade requirement of taking the titanium concentrate as the raw material can be reduced, so that the TiO2 ore dressing yield can be improved by ore dressing enterprises, the titanium resource rate is improved, and the environmental pollution caused by improving the titanium yield in the ore dressing process is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano titanium dioxide and titanium dioxide production, in particular to a method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium ore. Background Art

[0002] Titanium dioxide (chemical formula: TiO2) is a polycrystalline compound. There are three crystal forms in nature: rutile, anatase and brookite. In particular, rutile titanium dioxide has the highest refractive index among white pigments (anatase is the second highest). Titanium dioxide (main chemical composition: titanium dioxide, particle size 200-350nm, treated with organic, inorganic or composite coating) is currently the best and most commonly used white pigment, and is one of the most important inorganic chemical products. Titanium dioxide has the properties of a semiconductor. Its electrical conductivity increases rapidly with the increase of temperature, and it is also very sensitive to hypoxia. The average dielectric constant of rutile titanium dioxide is 114, and it has stable chemical properties and good thermal stability. Nano titanium dioxide (particle size 1-100nm) has a series of excellent properties (such as color effect, photocatalytic activity, shielding function against ultraviolet rays, high thermal conductivity, high magnetism, good transparency and excellent antibacterial properties). Both are widely used in industrial fields such as coatings, plastics, papermaking, electronics, water treatment, catalysis, rubber, ink, chemical fiber, ceramics, etc. There are two main methods for preparing nano titanium dioxide: physical method and chemical method. The physical method refers to the use of photoelectric technology combined with mechanical effects such as ball milling and spraying to refine the material to the nanometer scale, but the cost is high and cannot be mass-produced. The chemical method is subdivided into gas phase method, liquid phase method and solid phase method, but all have high requirements for titanium raw materials, complex processes, high preparation costs, and are difficult to industrialize.

[0003] The mature technology for wet production of titanium dioxide is sulfuric acid titanium dioxide production technology, and hydrochloric acid titanium dioxide production technology is under development. Titanium raw materials are mainly acid-soluble titanium slag and titanium concentrate. Sulfuric acid decomposes titanium minerals to obtain a mixed solution of titanium oxysulfate and titanium sulfate, and hydrochloric acid decomposes titanium minerals to obtain a titanium oxychloride solution. Other acid-soluble impurities are decomposed into soluble sulfates and chlorides, such as divalent iron salts, calcium salts, magnesium salts, etc. Undecomposed minerals are mixed in the solution in the form of solid impurities, which can be removed by filtering. The solution is called titanium liquid. Titanium liquid undergoes processes such as impurity removal, concentration increase, hydrolysis to prepare hydrated titanium dioxide, filtration, washing, calcination, and post-treatment to obtain pigment-grade titanium dioxide. However, the current limited production of high-titanium content resources and titanium-rich raw materials has restricted the further development of the titanium dioxide production industry. my country's Panxi-Xichang region is rich in vanadium-titanium magnetite resources. Its vanadium and titanium are present in polymetallic symbiotic deposits in the form of vanadium-titanium magnetite, accompanied by a small amount of valuable elements such as cobalt, chromium, and copper. Due to the characteristics of resource occurrence, titanium concentrate, iron concentrate and tailings are obtained through complex processes such as magnetic separation and flotation. About 50% of the titanium in vanadium-titanium magnetite enters the blast furnace with the iron concentrate after ore dressing. The tailings also contain a large amount of TiO2. In order to make full use of titanium resources, the titanium ore further selected from the iron tailings is called titanium middlings. Its typical TiO2 grade is about 36% to 38%, which is about 10% lower than the grade of titanium concentrate. It has a high impurity content and does not meet the industrial requirements for the direct production of sponge titanium, artificial rutile, titanium dioxide and high-titanium slag. Its economic efficiency is not high when used alone in existing industrial production, and it puts great pressure on environmental protection. Summary of the invention

[0004] The technical problem to be solved by the present invention is: how to provide a method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium medium ore, which can utilize titanium medium ore to produce nano titanium dioxide and rutile titanium dioxide for pigment, improve the resource utilization rate of titanium in vanadium titanium magnetite, expand the application field of by-products, and solve the problems of insufficient market supply of titanium concentrate and green and environmentally friendly production.

[0005] The technical solution of the present invention is: a method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium ore, comprising the following steps:

[0006] (1) grinding and microwave pre-activating the titanium ore raw material to obtain pre-activated titanium ore fine material;

[0007] (2) adding mother liquor roasting absorption acid into the chlorination leaching kettle, adding the pre-activated titanium ore fine material of step (1) into the chlorination leaching kettle under stirring and introducing the hydrogen chloride gas generated by the hydrochloric acid analysis system; using the dissolution heat of the hydrogen chloride gas to heat and perform acid hydrolysis to obtain a chlorinated slurry; adding iron powder and a deflocculating composite agent in the later stage of the acid hydrolysis to maintain the effective hydrochloric acid concentration in the kettle greater than 265 g / L, and recovering the acid hydrolysis tail gas generated during the acid hydrolysis process by using the hydrochloric acid analysis system;

[0008] (3) hot filtering the chlorinated slurry of step (2) to obtain leached residue and leached liquid; acid leaching the leached residue to prepare a porous silicon-titanium material, and fine filtering the leached liquid through the porous silicon-titanium material to obtain a finely filtered leached liquid;

[0009] (4) freezing and crystallizing the finely filtered leachate from step (3), and then filtering by pressure to obtain a ferrous chloride filter cake and a titanium-clearing solution; dissolving the ferrous chloride filter cake with hydrochloric acid produced by a hydrochloric acid analysis system, and then spray-roasting to obtain ferric oxide, and recovering hydrogen chloride with the hydrochloric acid analysis system;

[0010] (5) The titanium dioxide removal solution in step (4) is divided into two parts, one part is used to prepare nano titanium dioxide, and the other part is used to prepare rutile titanium dioxide;

[0011] (5.1) The steps for preparing nano titanium dioxide are:

[0012] a. Concentrating the clear titanium liquid to obtain concentrated titanium liquid and recovering the condensed acid;

[0013] b. The concentrated titanium liquid is subjected to self-seed hydrolysis to obtain nano-titanium dioxide precursor and recover condensed acid;

[0014] c. Filter the nano-titanium dioxide precursor with a membrane and wash it with the hydrochloric acid generated by the hydrochloric acid analysis system or the recovered condensed acid to obtain a clean filter material. The filtered hydrolysis mother liquor and washing liquid are returned to step (3) for fine filtration;

[0015] d. Wash the filter material and neutralize it with dilute ammonia water, then centrifuge and concentrate it and flash dry it to obtain powder;

[0016] e. Calcine the powder to obtain nano titanium dioxide and recover ammonium chloride;

[0017] (5.2) The steps for preparing rutile titanium dioxide are:

[0018] a. Concentrating the clear titanium liquid to obtain concentrated titanium liquid and recovering the condensed acid;

[0019] b. adding heterogeneous crystal nuclei to concentrated titanium solution to hydrolyze at normal pressure to obtain hydrated titanium dioxide and recover condensed acid;

[0020] c. Filtering the hydrated titanium dioxide and washing it with recovered condensed acid to obtain a hydrated titanium dioxide filter cake; spray roasting the hydrolysis mother liquor and washing liquid after the filtration to obtain iron oxide powder and mother liquor roasting absorption acid;

[0021] d. The hydrated titanium dioxide filter cake is calcined to obtain rutile titanium dioxide primary powder.

[0022] Furthermore, in step (1), the particle size of the pre-activated titanium ore fine material is less than 38 μm.

[0023] Furthermore, in step (2), the acid hydrolysis temperature is 90° C. and the acid hydrolysis time is 1.5-2.0 h.

[0024] Further, in step (2), at the end of the acid hydrolysis, Ti in the acid hydrolysis slurry 3+ It is 1.5~2g / L.

[0025] Furthermore, in step (5.1) a, the concentration of free hydrochloric acid in the concentrated titanium solution is 25-30 g / L, and the concentration of titanium ions is about 300 g / L calculated as TiO2.

[0026] In the present invention, according to the mineral coating characteristics of the titanium ore raw material, the titanium ore decomposed material used is a fine material that has been pre-activated by mechanochemical method and activated by microwave treatment through vertical mill grinding. The mineral particles undergo crushing, smashing, grinding, bending and other actions during the mechanical activation process, and the dielectric material during the microwave treatment process produces electronic polarization, atomic polarization, dipole steering polarization and interface polarization, resulting in particle refinement and structural changes, such as crystal transformation, recrystallization, amorphization, and the breaking of surface chemical bonds to produce unsaturated groups, free ions and electrons, etc., and new surfaces are generated, resulting in lattice defects, resulting in an increase in the internal energy of the mineral crystal, and being in an unstable chemically active state, and making many reactions that cannot occur under normal pressure and room temperature possible. Compared with ordinary titanium ore powder, it has higher surface energy and is easily acidified by chlorination leaching. The particle size of the titanium ore activated for chlorination leaching is controlled to D max <38μm.

[0027] The clear titanium liquid obtained through the steps of chlorination leaching, leaching slurry filtration, leaching liquid filtration and ferrous chloride crystallization separation is evaporated and concentrated, and the condensed acid is recovered to obtain a concentrated titanium liquid that meets the conditions for the hydrolysis preparation of nano titanium dioxide. The free acidity of the concentrated titanium liquid is 25-30g / L, and the titanium ion concentration (in terms of TiO2) is about 300g / L. Self-nucleation hydrolysis is carried out under the conditions of relatively low temperature (≤65°C) and relatively low hydrolysis rate of titanium ions (60% to 70%). Under the control conditions of low effective acidity, low temperature and low hydrolysis rate, the nucleation rate and growth rate of the crystal nucleus are relatively slow, so that the primary particles of the basic crystal grow to the range of several nanometers, avoiding the formation of large micelle flocculation particles.

[0028] The hydrolysis slurry containing the nano-titanium dioxide precursor that has been partially hydrolyzed is filtered and washed to obtain the purified nano-titanium dioxide precursor slurry and the unhydrolyzed hydrolysis mother liquor and the pickling liquid. The nanofiltration and washing are realized by using a nanofiltration element with a composite structure of a high-precision ceramic membrane-diatomaceous earth, activated carbon-high-precision ceramic membrane. The washing liquid is the condensed acid produced when the hydrochloric acid is analyzed or the titanium liquid is concentrated. Both are pure acids, which can strengthen the washing process and avoid the hydrolysis of impurities such as iron, and wash Fe 2+ , Fe 3+ Mg2+ , Ca 2+ and Al 3+ And other impurity ions.

[0029] The washed nano-titanium dioxide precursor slurry is neutralized with dilute ammonia water to neutralize the adsorbed and entrained HCl into ammonium chloride. After concentration and flash drying, the powder is heat treated for 1-1.5 hours in a tunnel kiln with a calcination temperature below 600°C to complete dehydration and complete conversion of rutile crystals. The ammonium chloride entrained in the powder sublimates at a temperature greater than 337.8°C and is crystallized and recovered in a cooling cabinet attached to the tunnel kiln flue (in essence, it is completely decomposed into ammonia and hydrogen chloride gas, and then combined into snowflake-shaped ammonium chloride crystals at low temperature). Since ammonium chloride first decomposes into ammonia and hydrogen chloride gas during the calcination process, it acts as a bulking agent to deagglomerate particles, solving the problem of severe agglomeration and particle growth of nano-powder materials during high-temperature dehydration and crystal material formation. At the same time, the chloride ions are deeply removed to meet the quality requirements of special nano-titanium dioxide products such as electronic ceramics. Nano-titanium dioxide can undergo conventional post-processing according to the needs of product use.

[0030] The incompletely hydrolyzed mother liquor and acid washing liquid of the hydrolysis slurry of the nano-titanium dioxide precursor are added to the leachate produced by the leaching slurry filtration for fine filtration to realize the recycling of components such as titanium, iron, and chlorine. Fine filtration removes the nano-titanium dioxide particles entrained in the hydrolysis mother liquor and the acid washing water, which can avoid the direct incorporation into the rutile titanium dioxide production system to affect the nucleation process and titanium-iron ratio of the hydrolysis process.

[0031] It is used to concentrate the titanium liquid in the production system of rutile titanium dioxide to produce pure condensed acid. The concentrated titanium liquid is hydrolyzed at normal pressure to prepare hydrated titanium dioxide by adding heterogeneous crystal nuclei. The heterogeneous crystal nuclei can reduce the energy of the system and promote Ti 4+ Hydrolysis is performed on heterogeneous crystal nuclei to increase the production rate of hydrated titanium dioxide particles. The heterogeneous crystal nuclei are amorphous silicon dioxide nano-spherical particles produced by the decomposition of mica by hydrochloric acid, with a particle size of several nanometers. The filtered and washed hydrated titanium dioxide filter cake is calcined in a rotary kiln to obtain the primary rutile titanium dioxide powder. The hydrolysis mother liquor is spray-roasted and absorbed to prepare low-end iron oxide powder and acid hydrolysis. The primary rutile titanium dioxide powder is ground, coated with aluminum silicon and then air flow crushed to prepare rutile titanium dioxide.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The comprehensive utilization of vanadium-titanium magnetite is realized, and the high-value-added nano-titanium dioxide and rutile titanium dioxide are prepared by chlorination leaching of titanium middlings. The production cost is low, hydrochloric acid is recycled, and the production process is environmentally friendly. In addition to using titanium middlings as raw materials, this method can also reduce the grade requirements for titanium concentrate as raw materials. Thus, mineral processing enterprises can increase the TiO2 mineral processing yield, increase the titanium resource rate, and avoid environmental pollution caused by increasing the titanium yield in the mineral processing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0035] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0036] Example 1

[0037] In this embodiment, the titanium ore raw material is Panzhihua titanium medium ore, with a TiO2 content of 37.51%, a FeO content of 38.57%, a Fe2O3 content of 7.20%, a P content of 0.051%, and a Dmax of ≤74 μm (200 mesh). The titanium concentrate powder is pre-activated and ground with a vertical mill and subjected to microwave activation heat treatment to obtain a pre-activated titanium medium ore fine material with a particle size of D 98 <35.3μm, Dmax<37μm (400 mesh).

[0038] Add 1400L of mother liquor roasting absorption acid (HCl: 320-330g / L) into a closed volume of 2m 3 The chlorination leaching reactor is put into the reactor and stirred, and then 700 kg of pre-activated titanium ore fine material is added into the chlorination leaching reactor and stirred to mix. The ore-acid ratio (mass-to-volume ratio) is 1:2.0.

[0039] The hydrogen chloride gas obtained by the hydrochloric acid analysis system is introduced, and the system is heated to 90°C by the heat of solution of the hydrogen chloride gas, and the system temperature is maintained to increase the acidity of the system, and the acid is stirred for 1.5 hours. The acid hydrolysis tail gas generated during the acid hydrolysis process is condensed and absorbed by the hydrochloric acid generated by the hydrochloric acid analysis system.

[0040] Add 13kg iron powder (elemental iron content 95%) to make Fe 3+ Reduction to Fe 2+ , add 320g of deflocculation composite agent (pre-dissolved), continue stirring for 0.5 hours, and ensure that Ti in the acid hydrolysis slurry is 3+ Reach 1.5-2g / L. Maintain the effective hydrochloric acid concentration of the acid hydrolysis reactor at 270g / L or above.

[0041] When the slurry temperature drops to 85℃, discharge the material and pump it to the silicon-titanium liquid supply tank, and then pump it to the acid-dissolved slurry membrane filter press for hot filtration. The filter cake of the acid-dissolved slurry is transported to the porous silicon-titanium composite material preparation section.

[0042] The acid solution from the acid solution slurry filtration is pumped to the acid solution transfer tank, and then pumped to the acid solution diaphragm filter press, and the fine filtrate is pumped to the crystallized titanium liquid intermediate storage tank.

[0043] Open the discharge valve of the intermediate storage tank of the crystalline titanium liquid, pump the refined filtrate into the closed crystalline titanium liquid tank, start stirring, turn on the ice water pump, and use ice water from the jacket to cool the crystalline titanium liquid. Pump the frozen crystalline titanium liquid into the chamber filter press, and stop feeding when the pressure in the filter press reaches 0.3MP. Open the compressed air valve and use compressed air to blow away the residual liquid in the ferrous chloride filter cake. The filtrate obtained is the clear titanium liquid. The detection indicators are: TiO2: 201.74g / L, Fe 2+ :42.60 / L,Cl - : 312.30g / L, effective acid concentration: 262.82g / L, free acid concentration: 72.65g / L, titanium ore acidification rate: 96.02%. The titanium clearing liquid is purple, and the stability is >500.

[0044] 600L of analytical acid (HCl: 200g / L) after the ferrous chloride filter cake is analyzed with hydrochloric acid is circulated and dissolved in a chamber filter press, and the prepared ferrous solution is pumped to the intermediate storage tank of the ferrous chloride solution in the regeneration acid spray roasting process to prepare high-quality ferric oxide powder and regeneration acid.

[0045] The clear titanium liquid used to prepare nano titanium dioxide is sent to a single-effect vacuum distillation system, and the mixed liquid is boiled and concentrated at low temperature under vacuum, with a concentration ratio of 70%. The concentrated titanium liquid is pumped to the concentrated titanium liquid storage tank, and the concentrated titanium liquid is tested for indicators (free acid concentration: 27.50g / L, TiO2: 286.2g / L, TFe: 59.84g / L). The steam and HCl generated by evaporation are condensed to obtain titanium liquid concentrated condensed acid (158.62g / L) through a condensation device.

[0046] In 1m 3 In the hydrolysis pot, add 700 liters of concentrated titanium liquid into the hydrolysis pot, start stirring, and rotate at 30r / min. Directly heat with saturated steam, raise the temperature to below 65℃, keep the hydrolysis and regularly detect until the hydrolysis rate (60% to 70%) of the titanium nano-titanium dioxide precursor (TiO2·2H2O) generated by continuous hydrolysis reaches the process requirement, and then terminate the hydrolysis. The hydrogen chloride gas and water vapor generated in the hydrolysis process are pumped to the falling film absorption system for tail gas absorption treatment, and the generated clean condensed acid is pumped into the secondary wash acid storage tank.

[0047] Open the discharge valve of the hydrolysis pot, and pump the hydrolyzed hydrated titanium dioxide slurry into the tubular membrane filtration washing system for nanofiltration and washing. The washing liquid uses the acid after hydrochloric acid analysis or the condensed acid produced when the titanium liquid is concentrated. Both are pure acids, which can strengthen the washing process and avoid the hydrolysis of impurities such as iron, and wash Fe 2+ , Fe 3+ Mg 2+ , Ca 2+ and Al 3+ And other impurity ions.

[0048] The washed nano-titanium dioxide precursor slurry is neutralized with dilute ammonia water to a pH value of 6-7, so that the adsorbed and entrained HCl is neutralized to ammonium chloride (NHCl). After centrifugal concentration and flash drying, the powder is calcined in a tunnel kiln at a temperature below 600°C for 1-1.5 hours for heat treatment to complete dehydration and complete conversion of rutile crystal form. The tunnel kiln is a push plate kiln, and the nano-titanium dioxide precursor is placed in a corundum sagger. The NH3Cl entrained in the powder sublimates at a temperature greater than 337.8°C and is crystallized and recovered in a cooling cabinet attached to the flue of the push plate kiln.

[0049] The hydrolysis slurry of the nano-titanium dioxide precursor is filtered through a membrane, and the titanium incomplete hydrolysis mother liquor and the acid washing liquid are pumped into the transfer tank of the acid hydrolysis liquid produced by the leaching slurry filtration, and the mixed liquid is subjected to the leaching liquid fine filtration.

[0050] The clean titanium liquid used to produce rutile titanium dioxide is metered and pumped into the single-effect vacuum distillation system. The mixed liquid is boiled and concentrated at low temperature under vacuum, and the concentration ratio is 70%. The concentrated titanium liquid is pumped to the concentrated titanium liquid storage tank, and the concentrated titanium liquid detection indicators (free acid concentration: 72.50g / L, Ti 3+ : 1.53 g / L, TiO2: 302.2 g / L, TFe: 57.84 g / L). The steam and HCl produced by evaporation are condensed by a condensation device to obtain titanium liquid concentrated condensed acid (152.42 g / L).

[0051] Add 60kg of 300-mesh mica powder and 150kg of 6M hydrochloric acid to 1M 3 The crystal nucleus preparation tank is stirred, leached and hydrolyzed at a temperature of 25-40°C, and the stirring reaction time is 2 hours. The white acid-insoluble matter (amorphous silicon dioxide) is filtered to obtain a precipitate. The precipitate (dry basis) is added with an equal mass of sodium hydroxide and stirred with pure water to form a slurry with a solid content of 10%, which is used as a heterogeneous crystal nucleus agent in the hydrolysis process of the rutile titanium powder preparation system.

[0052] Open the discharge valve and liquid pump of the concentrated titanium liquid storage tank, and pump 1400L of concentrated titanium liquid into the 2M 3 Hydrolysis pot.

[0053] Start the mixer at a speed of 30r / min, introduce saturated steam for direct heating, heat the concentrated titanium liquid to 90°C, quickly add 2L of seed slurry, use steam heating to raise the temperature to boiling of the hydrolyzed liquid and keep it warm for 30 minutes, and the solid product of titanium generated by continuous hydrolysis is hydrated titanium dioxide TiO2·2H2O. The hydrolysis rate is detected to be 99% before the hydrolysis is completed. Add 100g of lignocellulose to the hydrolysis pot and stir evenly. The hydrolyzed hydrated titanium dioxide slurry is cooled naturally to 60-70°C. Open the discharge valve of the hydrolysis pot and pump the hydrated titanium dioxide into the hydrated titanium dioxide storage tank with a hydrated titanium dioxide transfer pump for subsequent washing process. The hydrogen chloride gas and water vapor generated during the hydrolysis process are pumped to the falling film absorption system for tail gas absorption treatment, and a small amount of clean condensed acid is generated.

[0054] When the hydrated titanium dioxide slurry storage tank is in a stirring state, open the discharge valve and the diaphragm filter press feed valve, pump the hydrated titanium dioxide slurry into the diaphragm filter press through the feed pipe, and the filtrate, i.e. the hydrolysis mother liquor, is sent to the mother liquor concentration system; the filter cake is washed once and twice in the diaphragm filter press, and the washing acid comes from the concentrated condensed acid of the titanium hydrolysis mother liquor and the concentrated condensed acid of the titanium liquid, HCl≥240g / L, and does not contain impurities such as iron. After washing, the material is unloaded, and the hydrated titanium dioxide filter cake is sent to the calcination process.

[0055] Open the hydrolysis mother liquor storage tank, pump the hydrolysis mother liquor into the hydrolysis mother liquor concentration reactor, start the steam, heat it to boiling by indirect heat exchange with the jacket, concentrate it according to a concentration ratio of 30%, condense and recover the hydrolysis mother liquor condensed acid, pump it to the secondary wash acid storage tank, and pump the concentrated mother liquor to the concentrated mother liquor storage tank of the spray roasting section.

[0056] The outlet valve of the concentrated mother liquor storage tank is opened, and the concentrated mother liquor is sprayed into the roasting furnace, contacts with hot air at a temperature of 750-850℃, and reacts with O2 and H2O to decompose into H2O+HCl mixed gas+solid metal oxide. The absorption acid storage tank is opened, and the washing acid after washing the hydrated titanium dioxide filter cake is used as the absorption liquid of the falling film absorption system in the spray roasting section to produce regenerated acid, which is pumped into the regenerated acid storage tank for chlorination leaching with a regenerated acid concentration of 350.40g / L.

[0057] Adjust the rotary kiln speed to 0.3r / min, and turn on the exhaust fan at the kiln tail. When the temperature at the kiln tail reaches about 350-400℃, the hydrated titanium dioxide filter cake is fed through the screw conveyor and sent to the kiln tail for calcination. The residence time of the material in the calcination rotary kiln is about 7-8 hours. The first temperature zone is 350-750℃, the residence time is 2.8 hours, and the hydrated titanium dioxide undergoes the process of adsorption water removal, crystallization water removal, deacidification, and desulfurization; the second temperature zone is 750-880℃, the residence time is 2.2 hours, and the rutile crystal transformation process of titanium dioxide is completed; the third temperature zone is 880-930℃, the residence time is 2.4 hours, and the titanium dioxide particle growth process is completed. The titanium dioxide powder calcined at about 930℃ output from the calcining rotary kiln head is transferred to the air-cooled rotary kiln through the unloading device of the lower end cover of the kiln body to cool down to 60℃. The particle size is 0.2-0.35μm, the rutile content is greater than 99%, and the titanium dioxide content is 99.87%. This is the primary rutile titanium dioxide powder, which is conveyed by belt to the storage bin after calcination. The rotary kiln tail gas is sprayed, washed and heat-exchanged by the Venturi concentrator, absorbed by the first and second falling films, and defogged by the electric demister.

[0058] The initial rutile titanium dioxide can be used directly or processed as required:

[0059] The depolymerization and dispersion production process of the primary rutile titanium dioxide is as follows: the primary titanium dioxide from the storage bin after calcination is placed in the roller mill buffer hopper, first ground by the roller mill. Then sent to the Raymond mill buffer hopper, sent to the Raymond mill for grinding and Raymond mill self-contained classifier for sorting through the feed screw, qualified powder is sent to the wetting tank feed screw by the Raymond mill dust collector, added with desalted water and dispersant in the wetting tank for slurrying, and then pumped to the sand mill pre-storage tank, and then pumped to the first-level sand mill for sand milling, stirred in the feed transfer tank after sand milling, and then pumped to the second-level sand mill for sand milling, the slurry is pumped to the coating pre-tank, the pH of the slurry is adjusted to 4, TiO2: 300-320g / L.

[0060] The depolymerized and dispersed rutile titanium dioxide primary product is continuously coated with silicon and aluminum. The dispersed and depolymerized titanium dioxide slurry is metered and pumped into the surface treatment tank (coating tank). The slurry is heated to 95°C, and sodium silicate solution (concentration: 400g / L) is continuously added. Dilute sulfuric acid is added once to adjust the pH value to 9.3-10, mature, and then the pH is adjusted to 6.8-7.2 for multiple times, and mature. Then, sodium aluminate solution (concentration: 200g / L) is continuously added, the pH is adjusted to 6.8-7.2, mature and cool the slurry temperature to 70°C, and then the pH is adjusted to 4.5-5.0. Afterwards, the coated slurry is pumped to a box-type diaphragm filter press for filtration and washing.

[0061] The qualified filter cake is sent to the flash dryer feed hopper, and directly contacts with the high-temperature airflow generated by the hot air furnace in the dryer, so that the water evaporates quickly and the material is dried quickly. The dry powder enters the high-temperature bag filter with the hot airflow to recover TiO2, and is conveyed to the front silo of the steam powder by the spiral. The dried material is sent to the steam flow pulverizer, and the organic coating agent is added at the same time for the depolymerization and dispersion processing of the titanium dioxide product in the last process.

Claims

1. A method for preparing nano titanium dioxide and rutile titanium dioxide by chlorination leaching of titanium ore, characterized in that: The steps include: (1) grinding and microwave pre-activating the titanium ore raw material to obtain pre-activated titanium ore fine material; (2) adding mother liquor roasting absorption acid into the chlorination leaching kettle, adding the pre-activated titanium ore fine material of step (1) into the chlorination leaching kettle under stirring and introducing the hydrogen chloride gas generated by the hydrochloric acid analysis system; using the dissolution heat of the hydrogen chloride gas to heat and perform acid hydrolysis to obtain a chlorinated slurry; adding iron powder and a deflocculating composite agent in the later stage of the acid hydrolysis to maintain the effective hydrochloric acid concentration in the kettle greater than 265 g / L, and recovering the acid hydrolysis tail gas generated during the acid hydrolysis process by using the hydrochloric acid analysis system; (3) hot filtering the chlorinated slurry of step (2) to obtain leached residue and leached liquid; acid leaching the leached residue to prepare a porous silicon-titanium material, and fine filtering the leached liquid through the porous silicon-titanium material to obtain a finely filtered leached liquid; (4) freezing and crystallizing the finely filtered leachate from step (3), and then filtering by pressure to obtain a ferrous chloride filter cake and a titanium-clearing solution; dissolving the ferrous chloride filter cake with hydrochloric acid produced by a hydrochloric acid analysis system, and then spray-roasting to obtain ferric oxide, and recovering hydrogen chloride with the hydrochloric acid analysis system; (5) The titanium dioxide removal solution in step (4) is divided into two parts, one part is used to prepare nano titanium dioxide, and the other part is used to prepare rutile titanium dioxide; (5.1) The steps for preparing nano titanium dioxide are: a. Concentrating the clear titanium liquid to obtain concentrated titanium liquid and recovering the condensed acid; b. The concentrated titanium liquid is subjected to self-seed hydrolysis to obtain nano-titanium dioxide precursor and recover condensed acid; c. Filter the nano-titanium dioxide precursor with a membrane and wash it with the hydrochloric acid generated by the hydrochloric acid analysis system or the recovered condensed acid to obtain a clean filter material. The filtered hydrolysis mother liquor and washing liquid are returned to step (3) for fine filtration; d. Wash the filter material and neutralize it with dilute ammonia water, then centrifuge and concentrate it and flash dry it to obtain powder; e. Calcine the powder to obtain nano titanium dioxide and recover ammonium chloride; (5.2) The steps for preparing rutile titanium dioxide are: a. Concentrating the clear titanium liquid to obtain concentrated titanium liquid and recovering the condensed acid; b. adding heterogeneous crystal nuclei to concentrated titanium solution to hydrolyze at normal pressure to obtain hydrated titanium dioxide and recover condensed acid; c. Filtering the hydrated titanium dioxide and washing it with recovered condensed acid to obtain a hydrated titanium dioxide filter cake; spray roasting the hydrolysis mother liquor and washing liquid after the filtration to obtain iron oxide powder and mother liquor roasting absorption acid; d. The hydrated titanium dioxide filter cake is calcined to obtain rutile titanium dioxide primary powder.

2. The method according to claim 1, characterized in that In step (1), the particle size of the pre-activated titanium ore fine material is less than 38 μm.

3. The method according to claim 1, characterized in that In step (2), the acid hydrolysis temperature is 90° C. and the acid hydrolysis time is 1.5-2.0 h.

4. The method according to claim 1, characterized in that: In step (2), at the end of the acid hydrolysis, Ti in the acid hydrolysis slurry 3+ It is 1.5~2g / L.

5. The method according to claim 1, characterized in that In step (5.1) a, the concentration of free hydrochloric acid in the concentrated titanium solution is 25-30 g / L, and the concentration of titanium ions is about 300 g / L calculated as TiO2.

Citation Information

Patent Citations

  • Method for preparing artificial rutile from rock ore type titanium concentrate with high calcium and manganese content serving as raw material

    CN101935065A

  • Method for preparing titanium white

    CN102616842A

  • Method for preparation of titanium-rich material by leaching ilmenite through chlorination titanium white powder waste hydrochloric acid and comprehensive utilization of chloride process titanium white powder waste hydrochloric acid

    CN109825701A

  • Method for preparing primary titanium dioxide for pigment by decomposing vanadium titano-magnetite ironmaking slag with hydrochloric acid

    CN116002751A

  • Processing aqueous titanium solutions to titanium dioxide pigment

    US6548039B1