Porous water treatment material and preparation method thereof

By generating porous water treatment materials for iron vanadate-indium vanadate composite film on diatomaceous earth, the problems of low efficiency and high cost of organic polluted wastewater treatment in the prior art are solved, and the effect of photocatalytic degradation of organic pollutants is achieved. Suitable for a wide range of organic wastewater treatment.

CN118894572AActive Publication Date: 2024-11-05SHENYANG LIGONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410934624.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

In the prior art, when treating organic polluted wastewater, microbial treatment is easily affected by pollution, and adsorption materials cannot continue to be adsorbed after being saturated. Physical treatment can only transfer pollutants without degradation. Chemical treatment methods require the treatment of precipitated sludge, resulting in low efficiency. And the cost is high, it is difficult to promote.

Method used

Fixed pore diatomaceous earth is used as a support to form an iron vanadate-indium vanadate composite film on the surface and pores, and photocatalyzed organic pollutants to form porous water treatment materials, with a large adsorption capacity and the ability to continuously remove organic pollutants.

Benefits of technology

It achieves the effect of continuously removing organic pollutants in water under light. The material density is lower than that of water, and is easy to separate and recycle. It is suitable for the treatment of various organic wastewater, improving treatment efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a porous water treatment material and a preparation method thereof, and belongs to the field of environmental pollution purification materials. The method comprises the main preparation steps of diatomite pore fixing, vanadium-iron-indium solution preparation and membrane deposition. The preparation method comprises the following steps: by taking fixed-pore diatomite as a carrier material, generating a ferric vanadate-indium oxide composite film on the surface of the diatomite and in pores. The porous water treatment material has relatively large adsorption capacity and can adsorb organic pollutants in water; the ferric vanadate-indium oxide composite film has the activity of degrading organic pollutants under illumination. The porous water treatment material can be quickly separated from water and recycled after water treatment is completed, and has a wide application prospect in the field of treatment of various organic wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental pollution purification materials, and in particular relates to a porous water treatment material and a preparation method thereof. Background Art

[0002] Industrial and civil wastewater contains a wide variety of pollutants, among which organic pollutants are more harmful to the environment and human health. Such wastewater must be deeply purified to avoid polluting the environment.

[0003] There are many methods for treating organic polluted wastewater, such as the common biochemical treatment technology, but the key microorganisms in biochemical technology are easily affected by toxic and harmful organic pollutants, and the wastewater treatment cannot meet satisfactory standards. Adsorption materials can effectively remove pollutants in water, but the biggest problem of such materials is that they have a certain adsorption saturation capacity. When the material is saturated with adsorption, it can no longer adsorb pollutants. There are also physical treatment methods, mainly including adsorption and membrane separation. However, the physical method only transfers the pollutants in the organic wastewater, and does not fundamentally degrade them to achieve the purpose of eliminating pollutants. In addition, the treatment efficiency is low, the amount of material consumed is large, resulting in high costs, and it is difficult to promote and use. In addition, there are chemical treatment methods, mainly including chemical flocculation and chemical oxidation. The chemical coagulation method is to add a certain amount of flocculant to the wastewater, and produce flocculation with the organic matter in the organic wastewater to generate precipitation or suspension to achieve the purpose of separation. This method is more economical and effective in the treatment of organic wastewater, but the precipitated sludge produced needs further treatment. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a porous water treatment material, which can be used in the photocatalytic purification process of organic pollutants in sewage.

[0005] The technical solution adopted by the present invention is:

[0006] A porous water treatment material is prepared by the above method, wherein the bulk density of the porous water treatment material is 0.65-0.68 g / cm 3 Specific surface area 66~69m 2 / g, pore volume 0.73~0.77cm 3 / g.

[0007] Furthermore, the porous water treatment material maintains stable structure and performance at temperatures below 450°C.

[0008] A method for preparing the above-mentioned porous water treatment material comprises the following process steps:

[0009] Step 1: Diatomaceous earth hole setting

[0010] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0011] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 550-560° C. for 3 h, and cool to room temperature to obtain diatomite with fixed pores;

[0012] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0013] 13-17 g of ferrous sulfate, 11-13 g of sodium metavanadate, and 8-9.5 g of indium nitrate were added to 130 mL of pure water, and stirred to form solution A; 5-6 g of emulsifier Tween 60 and 3-3.6 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol, and stirred to form solution B; solution B was slowly added to solution A, and kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution;

[0014] Step 3: Film Deposition

[0015] The fixed-pore diatomaceous earth prepared in step 1 is mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 220-250° C. for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C is dried at 190° C. for 22 hours, then calcined at 460-510° C. for 5 hours, and cooled to room temperature to obtain a porous water treatment material.

[0016] Furthermore, the diatomaceous earth in step (1) has a particle size of 18 to 22 mm and a bulk density of 0.6 g / cm 3 , specific surface area 75m 2 / g, pore volume 0.82cm 3 / g.

[0017] Furthermore, an iron vanadate-indium oxide composite film is formed on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), and the composite film is firmly bonded to the diatomite.

[0018] Furthermore, the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of iron vanadate in the porous water treatment material is 3.8% to 4.3%, and the mass percentage of indium oxide in the porous water treatment material is 2.7% to 3.1%. The relative mass ratio of iron vanadate and indium oxide is the key to ensuring the stability of the material and the photocatalytic performance.

[0019] Compared with the prior art, the porous water treatment material and preparation method of the present invention have the following advantages: the present invention uses fixed-pore diatomite as a carrier material to generate an iron vanadate-indium oxide composite film on the surface of the diatomite and inside the pores. The porous water treatment material has a large adsorption capacity and can adsorb organic pollutants in water; under light, the iron vanadate-indium oxide composite film coated on the porous water treatment material has the activity of degrading organic pollutants, so that the material has the performance of continuously removing organic pollutants from water. The porous water treatment material has a lower density than water, and can be quickly separated from water and recycled after water treatment is completed, and has broad application prospects in various organic wastewater treatment fields. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples where no specific conditions are indicated are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0021] Unless otherwise specified, all chemical raw materials mentioned are pure materials.

[0022] Example 1

[0023] A method for preparing a porous water treatment material comprises the following process steps:

[0024] Step 1: Diatomaceous earth hole setting

[0025] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0026] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 550° C. for 3 h, and cool to room temperature to obtain diatomaceous earth with fixed pores.

[0027] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0028] 13 g of ferrous sulfate, 11 g of sodium metavanadate and 8 g of indium nitrate were added to 130 mL of pure water and stirred to form solution A; 5 g of emulsifier Tween 60 and 3 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol and stirred to form solution B; solution B was slowly added to solution A and kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution.

[0029] Step 3: Film Deposition

[0030] The diatomaceous earth prepared in step 1 was mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 220°C for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C was dried at 190°C for 22 hours, then calcined at 460°C for 5 hours, and cooled to room temperature to obtain a porous water treatment material, wherein the bulk density of the porous water treatment material is 0.65 g / cm 3 , specific surface area 69m 2 / g, pore volume 0.77cm 3 / g.

[0031] An iron vanadate-indium oxide composite film is generated on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), wherein the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of the iron vanadate in the porous water treatment material is 3.8%, and the mass percentage of indium oxide in the porous water treatment material is 2.7%.

[0032] Example 2

[0033] A method for preparing a porous water treatment material comprises the following process steps:

[0034] Step 1: Diatomaceous earth hole setting

[0035] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0036] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 550° C. for 3 h, and cool to room temperature to obtain diatomaceous earth with fixed pores.

[0037] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0038] 14 g of ferrous sulfate, 11.5 g of sodium metavanadate, and 8.3 g of indium nitrate were added to 130 mL of pure water and stirred to form solution A; 5.2 g of emulsifier Tween 60 and 3.1 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol and stirred to form solution B; solution B was slowly added to solution A, and the mixture was kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution.

[0039] Step 3: Film Deposition

[0040] The diatomaceous earth prepared in step 1 was mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 225°C for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C was dried at 190°C for 22 hours, then calcined at 470°C for 5 hours, and cooled to room temperature to obtain a porous water treatment material, wherein the bulk density of the porous water treatment material is 0.66 g / cm 3 , specific surface area 68m 2 / g, pore volume 0.76cm 3 / g.

[0041] An iron vanadate-indium oxide composite film is generated on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), wherein the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of the iron vanadate in the porous water treatment material is 3.9%, and the mass percentage of indium oxide in the porous water treatment material is 2.8%.

[0042] Example 3

[0043] A method for preparing a porous water treatment material comprises the following process steps:

[0044] Step 1: Diatomaceous earth hole setting

[0045] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0046] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 555° C. for 3 h, and cool to room temperature to obtain diatomaceous earth with fixed pores.

[0047] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0048] 15 g of ferrous sulfate, 12 g of sodium metavanadate, and 8.8 g of indium nitrate were added to 130 mL of pure water and stirred to form solution A; 5.5 g of emulsifier Tween 60 and 3.3 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol and stirred to form solution B; solution B was slowly added to solution A, and the mixture was kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution.

[0049] Step 3: Film Deposition

[0050] The diatomite prepared in step 1 was mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 235°C for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C was dried at 190°C for 22 hours, then calcined at 480°C for 5 hours, and cooled to room temperature to obtain a porous water treatment material, wherein the bulk density of the porous water treatment material is 0.66 g / cm 3 , specific surface area 67m 2 / g, pore volume 0.75cm 3 / g.

[0051] An iron vanadate-indium oxide composite film is generated on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), wherein the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of the iron vanadate in the porous water treatment material is 4.0%, and the mass percentage of indium oxide in the porous water treatment material is 2.9%.

[0052] Example 4

[0053] A method for preparing a porous water treatment material comprises the following process steps:

[0054] Step 1: Diatomaceous earth hole setting

[0055] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0056] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 560° C. for 3 h, and cool to room temperature to obtain diatomaceous earth with fixed pores.

[0057] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0058] 16 g of ferrous sulfate, 12.3 g of sodium metavanadate, and 9.2 g of indium nitrate were added to 130 mL of pure water and stirred to form solution A; 5.8 g of emulsifier Tween 60 and 3.5 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol and stirred to form solution B; solution B was slowly added to solution A, and the mixture was kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution.

[0059] Step 3: Film Deposition

[0060] The diatomaceous earth prepared in step 1 was mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 240°C for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C was dried at 190°C for 22 hours, then calcined at 495°C for 5 hours, and cooled to room temperature to obtain a porous water treatment material, wherein the bulk density of the porous water treatment material is 0.67 g / cm 3 , specific surface area 67m 2 / g, pore volume 0.75cm 3 / g.

[0061] An iron vanadate-indium oxide composite film is generated on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), wherein the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of the iron vanadate in the porous water treatment material is 4.2%, and the mass percentage of the indium oxide in the porous water treatment material is 3.0%.

[0062] Example 5

[0063] A method for preparing a porous water treatment material comprises the following process steps:

[0064] Step 1: Diatomaceous earth hole setting

[0065] (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A;

[0066] (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 560° C. for 3 h, and cool to room temperature to obtain diatomaceous earth with fixed pores.

[0067] Step 2: Preparation of Vanadium-Iron-Indium Solution

[0068] 17 g of ferrous sulfate, 13 g of sodium metavanadate, and 9.5 g of indium nitrate were added to 130 mL of pure water and stirred to form solution A; 6 g of emulsifier Tween 60 and 3.6 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol and stirred to form solution B; solution B was slowly added to solution A, and the mixture was kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution.

[0069] Step 3: Film Deposition

[0070] The diatomite prepared in step 1 was mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 250°C for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C was dried at 190°C for 22 hours, then calcined at 510°C for 5 hours, and cooled to room temperature to obtain a porous water treatment material, wherein the bulk density of the porous water treatment material is 0.68 g / cm 3 , specific surface area 66m 2 / g, pore volume 0.73cm 3 / g.

[0071] An iron vanadate-indium oxide composite film is generated on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), wherein the iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of the iron vanadate in the porous water treatment material is 4.3%, and the mass percentage of the indium oxide in the porous water treatment material is 3.1%.

Claims

1. A porous water treatment material, characterized in that: The bulk density of the porous water treatment material is 0.65-0.68 g / cm 3 Specific surface area 66~69m 2 / g, pore volume 0.73~0.77cm 3 / g.

2. A porous water treatment material according to claim 1, characterized in that: The porous water treatment material maintains stable structure and performance at temperatures below 450°C.

3. A method for preparing the porous water treatment material according to claim 1 or 2, characterized in that: The process includes the following steps: Step 1: Diatomaceous earth hole setting (1) Add 680 mL of 0.25 mol / L hydrochloric acid solution and 50 g of diatomaceous earth to a flask, place in a constant temperature water bath at 85° C. and stir for 120 min. After cooling, filter, wash with pure water and filter to obtain solid A; (2) Repeat the above step twice with solid A to obtain solid B; dry solid B at 180° C. for 15 h, then calcine at 550-560° C. for 3 h, and cool to room temperature to obtain diatomite with fixed pores; Step 2: Preparation of Vanadium-Iron-Indium Solution 13-17 g of ferrous sulfate, 11-13 g of sodium metavanadate, and 8-9.5 g of indium nitrate were added to 130 mL of pure water, and stirred to form solution A; 5-6 g of emulsifier Tween 60 and 3-3.6 g of polyethylene glycol with a molecular weight of 6000 were added to 60 mL of ethanol, and stirred to form solution B; solution B was slowly added to solution A, and kept warm in a constant temperature water bath at 35° C. for 30 minutes to obtain a vanadium-iron-indium solution; Step 3: Film Deposition The fixed-pore diatomaceous earth prepared in step 1 is mixed with the vanadium-iron-indium solution, transferred into a stainless steel hydrothermal reactor, reacted at 220-250° C. for 72 hours, filtered after cooling, and then filtered after washing with pure water to obtain a solid C; the solid C is dried at 190° C. for 22 hours, then calcined at 460-510° C. for 5 hours, and cooled to room temperature to obtain a porous water treatment material.

4. The method for preparing a porous water treatment material according to claim 3, characterized in that: The diatomaceous earth in step (1) has a particle size of 18 to 22 mm and a bulk density of 0.6 g / cm 3 , specific surface area 75m 2 / g, pore volume 0.82cm 3 / g.

5. The method for preparing a porous water treatment material according to claim 3, characterized in that: An iron vanadate-indium oxide composite film is formed on the surface and inside the pores of the fixed-pore diatomite prepared in step (1), and the composite film is firmly bonded to the diatomite.

6. The method for preparing a porous water treatment material according to claim 5, characterized in that: The iron vanadate-indium oxide composite film is composed of two photocatalytically active substances, iron vanadate and indium oxide, wherein the mass percentage of iron vanadate in the porous water treatment material is 3.8% to 4.3%, and the mass percentage of indium oxide in the porous water treatment material is 2.7% to 3.1%. The relative mass ratio of iron vanadate and indium oxide is the key to ensuring the stability of the material and the photocatalytic performance.

Citation Information

Patent Citations

  • Manganese oxide and infusorial earth composite adsorbent for treating lead-containing wastewater and preparation method

    CN102941060A

  • Preparation method of MoS2 / SrFe12O19 composite magnetic photocatalyst

    CN108452813A

  • Preparation method of air purifying material

    CN109012169A

  • Preparation method for light kieselguhr water treatment materials

    CN109231340A