Multi-dimensional assembled nano thermal insulation material and preparation method thereof

By using high aspect ratio nanofibers and magnesium aluminum spinel nanopowder combined with high-temperature binders and supercritical drying technology, multidimensional assembled nano-insulation materials were prepared, solving the problems of insufficient insulation performance and complicated preparation of existing nanofiber insulation materials, and achieving excellent insulation and mechanical properties at high temperatures.

CN118894700AActive Publication Date: 2024-11-05BEIJING UNIV OF CHEM TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410945761.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The micron-scale macroporous structure of existing nanofiber insulation materials cannot effectively restrict gas heat transfer, resulting in insufficient insulation performance. Furthermore, traditional preparation methods are cumbersome and difficult to scale up for production.

Method used

High aspect ratio nanofibers and magnesium aluminum spinel nanoparticles are used as the framework structure. Combined with high-temperature binders and supercritical drying technology, multidimensional assembled nano-insulating materials are prepared to avoid the sol-gel process and form a high-strength framework with a bird's nest-like structure.

Benefits of technology

It improves the mechanical strength and thermal insulation performance of nanofiber insulation materials, enabling them to be used at high temperatures of 1400℃, simplifies the preparation process, and reduces the thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945570280000171
    Figure BDA0004945570280000171
  • Figure BDA0004945570280000181
    Figure BDA0004945570280000181
Patent Text Reader

Abstract

The invention relates to a multi-dimensional assembled nano thermal insulation material and a preparation method thereof. The method comprises the following steps: uniformly dispersing nanofibers with a high length-diameter ratio, magnesium aluminate spinel nanopowder and nano silicon carbide with water to obtain dispersed slurry; adding a high-temperature adhesive into the dispersed slurry, uniformly dispersing, and aging to obtain wet gel; the high-temperature adhesive is one or more of a calcium aluminate cement gelling agent, a zirconium oxide-calcium phosphate composite sol gelling agent and a calcium aluminosilicate cement gelling agent; the wet gel is sequentially subjected to solvent replacement and supercritical drying, and the multi-dimensional assembled nanometer heat insulation material is prepared. The macroporous structure of the nanofiber is improved, gas-phase heat transfer in the heat insulation material is limited, the problem of insufficient mechanical strength of the nanofiber material can be effectively solved, and the mechanical and thermal properties of the nanofiber heat insulation material can be comprehensively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiber thermal insulation materials, and in particular relates to a multi-dimensionally assembled nano thermal insulation material and a preparation method thereof. Background Art

[0002] Nanofiber thermal insulation materials, with the characteristics of light weight, high temperature resistance and low thermal conductivity, have become a research hotspot in the field of nano thermal insulation materials. However, current nanofiber thermal insulation materials are all assembled and prepared with nanofibers as the skeleton. The micron-scale macroporous structure inside the material cannot effectively limit the heat transfer of the gas, making the thermal insulation performance of the material seriously insufficient.

[0003] In the prior art, there are reports that the method of doping aerogel nanoparticles to improve the pore structure has been proposed, and the thermal insulation performance of the material has been effectively improved. However, at this stage, silica aerogel particles are used as skeleton insulation fillers. The temperature resistance of silica aerogel is seriously insufficient, and the material preparation requires the use of a sol-gel process. The entire composite material preparation process is cumbersome. At the same time, the preparation of nanofibers is all prepared by freeze-drying, and the process is not easy to scale up. It is urgent to develop a simple and effective method for preparing high-temperature resistant nanofiber aerogel composite insulation materials.

[0004] In summary, it is very necessary to provide a multi-dimensionally assembled nano thermal insulation material and a preparation method thereof. Summary of the invention

[0005] In order to solve one or more technical problems existing in the prior art, the present invention provides a multi-dimensionally assembled nano thermal insulation material and a preparation method thereof.

[0006] In a first aspect, the present invention provides a method for preparing a multi-dimensionally assembled nano thermal insulation material, the method comprising the following steps:

[0007] (1) using water to uniformly disperse nanofibers with a high aspect ratio, magnesium aluminum spinel nanopowder, and nano silicon carbide to obtain a dispersed slurry;

[0008] (2) adding a high temperature adhesive to the dispersed slurry and dispersing it evenly, and then aging it to obtain a wet gel; the high temperature adhesive is one or more of a calcium aluminate cement gelling agent, a zirconium oxide-calcium phosphate gelling agent, and a calcium aluminosilicate cement gelling agent;

[0009] (3) The wet gel is subjected to solvent replacement and supercritical drying in sequence to obtain a multi-dimensionally assembled nano thermal insulation material.

[0010] Preferably, the nanofiber is one or more of zirconium oxide nanofiber, magnesium aluminum spinel nanofiber, zirconium silicate nanofiber, mullite nanofiber and aluminum oxide nanofiber.

[0011] Preferably, the aspect ratio of the nanofiber is (200-10000):1; and / or the particle size of the magnesium aluminum spinel nanopowder is 20nm-200nm.

[0012] Preferably, the mass ratio of the nanofiber to the magnesium aluminum spinel nanopowder is (1-9):1; and / or the mass amount of the nano-silicon carbide is 4-8% of the sum of the mass amounts of the nanofiber and the magnesium aluminum spinel nanopowder.

[0013] Preferably, the sum of the mass percentages of nanofibers and magnesium aluminum spinel nanopowder in the dispersed slurry is 10-20%; and / or the mass amount of the high-temperature adhesive in step (2) is 5-20% of the mass amount of the nanofibers in step (1).

[0014] Preferably, the aging temperature is 60° C. to 90° C., and the aging time is 12 h to 48 h.

[0015] Preferably, the number of solvent replacements is 3 to 5 times; the solvent replacement uses a cyclohexane / ethanol mixed solvent as the solvent, preferably, the cyclohexane / ethanol mixed solvent is a mixture of n-hexane and ethanol in a volume ratio of 1:(1 to 3); and / or the supercritical drying time is 48 to 96 hours.

[0016] Preferably, in step (1), rare earth high entropy ceramic nanofibers are also added, and the mass ratio of the rare earth high entropy ceramic nanofibers to the magnesium aluminum spinel nanopowder is 1:(1-2).

[0017] Preferably, the rare earth high entropy ceramic nanofibers are rare earth zirconate high entropy ceramic nanofibers A2Zr2O7 and / or rare earth hafnium salt high entropy ceramic nanofibers B2Hf2O7; A is any five of the rare earth elements La, Sr, Ce, Er, Y and Yb, and the sum of the atomic molar percentages of each rare earth element is 100%, and the atomic molar percentages of each rare earth element are equal, or the atomic molar percentages differ by no more than 1 to 3%; B is any five of the rare earth elements Nd, Sm, Eu, Gd, Dy and Er, and the sum of the atomic molar percentages of each rare earth element is 100%, and the atomic molar percentages of each rare earth element are equal, or the atomic molar percentages differ by no more than 1 to 3%.

[0018] In a second aspect, the present invention provides a multi-dimensionally assembled nano thermal insulation material prepared by the preparation method described in the first aspect of the present invention.

[0019] Compared with the prior art, the present invention has at least the following beneficial effects:

[0020] The present invention uses high temperature resistant magnesium aluminum spinel nano powder as a pore structure regulator to improve the macroporous structure of nanofibers, limit the gas phase heat transfer inside the thermal insulation material, and directly introduces the nanopore regulator to avoid the cumbersome sol-gel process, making the material preparation process more convenient; the present invention uses high temperature resistant high aspect ratio nanofibers as skeleton structural components, and utilizes the winding effect of aspect ratio fibers to form a high-strength nanofiber skeleton with a bird's nest structure, which can effectively solve the problem of insufficient mechanical strength of nanofiber materials; in addition, the present invention avoids the secondary high temperature treatment process of the traditional nanofiber aerogel material molding process by introducing a high temperature inorganic gelling agent as a high temperature adhesive, and can comprehensively improve the mechanical and thermal properties of nanofiber thermal insulation materials; the multi-dimensionally assembled nano thermal insulation material prepared by the present invention can withstand a high temperature of 1400°C. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In a first aspect, the present invention provides a method for preparing a multi-dimensionally assembled nano thermal insulation material, the method comprising the following steps:

[0023] (1) Using water to evenly disperse high aspect ratio nanofibers, magnesium aluminum spinel nanopowder and nano silicon carbide (also referred to as silicon carbide nanopowder) to obtain a dispersed slurry; in the present invention, the particle size (average particle size) of the nano silicon carbide is 50 to 100 nm; in the present invention, the magnesium aluminum spinel nanopowder is also referred to as nano magnesium aluminum spinel; in the present invention, specifically, for example, a certain ratio of high aspect ratio nanofibers, magnesium aluminum spinel nanopowder and nano silicon carbide are stirred and dispersed in water to obtain a dispersed slurry, which is a raw material for assembling a multi-dimensional nanofiber thermal insulation skeleton; the present invention does not specifically limit the stirring and dispersing method, and does not specifically limit the amount of silicon carbide added, which can be conventionally selected by those skilled in the art;

[0024] (2) adding a high-temperature adhesive to the dispersed slurry and dispersing it uniformly, and then aging it to obtain a wet gel; the high-temperature adhesive is one or more of calcium aluminate cement gelling agent (i.e. calcium aluminate cement), zirconium oxide-calcium phosphate composite sol gelling agent and calcium aluminosilicate cement gelling agent (i.e. calcium aluminosilicate cement); the present invention does not specifically limit calcium aluminate cement and calcium aluminosilicate cement, and products that can be directly purchased can be used; in the present invention, calcium aluminosilicate cement refers to a silicate cement with calcium aluminosilicate as the main component; in the present invention, the zirconium oxide-calcium phosphate composite sol gelling agent is prepared by mixing zirconium oxide sol and calcium phosphate sol in a mass ratio of 1:1, the solid content of the zirconium oxide sol is 20-25wt%, and the solid content of the calcium phosphate sol is 20-25wt%; in the present invention, adding a high-temperature adhesive to the dispersed slurry and stirring and dispersing it uniformly, and then subjecting it to high-temperature shrinkage aging to obtain a wet gel;

[0025] (3) The wet gel is subjected to solvent replacement and supercritical drying in sequence to obtain a multi-dimensionally assembled nano-insulating material; in the present invention, supercritical drying is carried out in a supercritical drying kettle, for example, supercritical carbon dioxide drying. The present invention does not specifically limit the conditions of supercritical drying, which is a conventional technology in the field; the present invention provides a method for preparing a nanofiber-reinforced composite insulating material based on magnesium-aluminum spinel, and the obtained multi-dimensionally assembled nano-insulating material is also recorded as a high-temperature resistant composite insulating material or a high-temperature resistant nanofiber aerogel composite insulating material.

[0026] The present invention uses high temperature resistant magnesium aluminum spinel nanopowder as a pore structure regulator to improve the macroporous structure of nanofibers and limit the gas phase heat transfer inside the thermal insulation material. At the same time, the method of directly introducing the nanopore regulator can avoid the cumbersome sol-gel process, and the material preparation process is more convenient; the present invention uses high temperature resistant high aspect ratio nanofibers as skeleton structural components, and utilizes the entanglement effect of aspect ratio fibers to form a high-strength nanofiber skeleton with a bird's nest structure, which can effectively solve the problem of insufficient mechanical strength of nanofiber materials; in addition, the present invention avoids the secondary high temperature treatment process of the traditional nanofiber aerogel material molding process by introducing a high temperature inorganic gelling agent (calcium aluminate cement gelling agent, zirconium oxide-calcium phosphate composite sol gelling agent and / or calcium aluminosilicate cement gelling agent) as a high temperature adhesive, which can comprehensively improve the mechanical and thermal properties of nanofiber thermal insulation materials. This is because the present invention has found that these inorganic gelling agents can make the dispersed slurry of the present invention form a firm gel at a relatively low temperature. The present invention discloses a novel nanofiber aerogel having a high temperature resistance and low thermal conductivity, which further reduces the thermal conductivity of the entire material, thereby facilitating the improvement of the thermal insulation performance of the material. In contrast, the traditional high-temperature adhesives such as silica sol and aluminum dihydrogen phosphate have weak hydration resistance, and generally organic gelling agents are added and / or high-temperature treatment is performed to solidify and enhance the material performance, which increases the production cost and process complexity. In addition, the temperature resistance of silica sol is limited, and aluminum dihydrogen phosphate is prone to expand during high-temperature curing to produce an uneven macroporous structure, which reduces the overall mechanical and thermal properties of the material. In addition, the secondary high-temperature treatment easily causes the pore structure of the nanofiber aerogel material to partially collapse or shrink, thereby reducing the porosity of the material. The reduction in porosity will lead to an increase in the thermal conductivity of the material and a decrease in the thermal insulation performance. The multi-dimensionally assembled nano thermal insulation material prepared by the present invention can withstand a high temperature of 1400°C.

[0027] According to some preferred embodiments, the nanofibers are one or more of zirconium oxide nanofibers, magnesium aluminum spinel nanofibers, zirconium silicate nanofibers, mullite nanofibers and aluminum oxide nanofibers. Preferably, the nanofibers are mullite nanofibers, magnesium aluminum spinel nanofibers, aluminum oxide nanofibers, zirconium silicate nanofibers and zirconium oxide fibers, etc. These nanofibers have excellent temperature resistance, all of which are not lower than 1300°C. The present invention does not specifically limit the source of these nanofibers, and may use products that can be directly purchased or products prepared by existing methods.

[0028] According to some preferred embodiments, the aspect ratio (average aspect ratio) of the nanofiber is (200-10000): 1 (e.g., 200: 1, 1000: 1, 2000: 1, 3000: 1, 4000: 1, 5000: 1, 6000: 1, 7000: 1, 8000: 1, 9000: 1 or 10000: 1); and / or the particle size (average particle size) of the magnesium aluminum spinel nanopowder is 20nm-200nm (e.g., 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 2010, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400 90 or 200nm); in the present invention, preferably, the aspect ratio of the nanofiber is 200:1 to 10000:1. The present invention finds that if the aspect ratio of the nanofiber is too small, it is difficult to form a skeleton structure, and if the aspect ratio is too large, the pore structure size is difficult to control, which will lead to the existence of a large number of micron-sized pores; in the present invention, the magnesium aluminum spinel has a stable crystal structure and good temperature resistance. As a high-temperature resistant pore structure regulator, it is preferred that the particle size is 20 to 200nm. The present invention finds that if the particle size of the magnesium aluminum spinel nanopowder is too small, it is difficult to effectively support the pore structure and the skeleton structure is unstable. If the particle size of the magnesium aluminum spinel nanopowder is too large, the pore structure regulation efficiency will be low.

[0029] According to some preferred embodiments, the mass ratio of the nanofibers to the magnesium aluminum spinel nanopowder is (1-9):1 (for example, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1); and / or the mass amount of the nano-silicon carbide is 4-8% (for example, 4%, 5%, 6% or 8%) of the sum of the mass amounts of the nanofibers and the magnesium aluminum spinel nanopowder.

[0030] According to some preferred embodiments, the sum of the mass percentages of the nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 10-20% (for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%); and / or the mass amount of the high temperature adhesive in step (2) is 5-20% (for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%) of the mass amount of the nanofibers in step (1). 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%); in the present invention, the amount of the high-temperature adhesive is preferably 5-20%. If the amount of the high-temperature adhesive is too large, the high-temperature adhesive will form its own cluster structure, the surface energy of the nano-component will be reduced, the material will be prone to shrinkage at high temperature, and the temperature resistance of the material will be reduced; at the same time, if the amount of the high-temperature adhesive is too large, the solid-phase thermal conductivity of the material will increase, and the nanofibers will also undergo local agglomeration, resulting in a significant increase in the macroscopic equivalent thermal conductivity of the material.

[0031] According to some preferred embodiments, the aging temperature is 60°C to 90°C (for example, 60°C, 70°C, 80°C or 90°C), and the aging time is 12h to 48h (for example, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46 or 48h). In the present invention, the temperature for aging to form a wet gel is preferably 60-90°C. If aging is carried out at a low temperature below 60°C, the aging efficiency will be low and the skeleton will be difficult to effectively strengthen. If aging is carried out at a high temperature above 90°C, the temperature is too high, which will cause air pressure to be generated and destroy the structural stability of the material.

[0032] According to some preferred embodiments, the number of solvent replacement is 3 to 5 times (for example, 3, 4 or 5 times), so as to ensure that the aqueous solution is completely replaced; in the present invention, preferably, the time for each solvent replacement is 18 to 30 hours; the solvent replacement uses a cyclohexane / ethanol mixed solvent as the solvent, and preferably, the cyclohexane / ethanol mixed solvent is a mixture of n-hexane and ethanol in a volume ratio of 1: (1 to 3) (for example, 1: 1, 1: 1.5, 1: 2, 1: 2.5 or 1: 3); in the present invention, preferably, a cyclohexane / ethanol mixed solvent is used as the solvent for solvent replacement, and the mixed use of the two can ensure the uniformity and thoroughness of the solvent replacement while protecting the nanostructure, and the use of a cyclohexane and ethanol mixed solvent in a volume ratio of 1: (1 to 3) for solvent replacement can effectively prevent the internal structure from cracking during the replacement process, and can better control the porosity and pore size distribution of the material, thereby improving the mechanical properties and thermal properties of the nano-insulation material.

[0033] According to some preferred embodiments, the supercritical drying time is 48 to 96 hours (eg, 48, 60, 72, 84 or 96 hours), which can ensure that the material is completely dried and avoid damage to the skeleton.

[0034] According to some preferred embodiments, in step (1), rare earth high entropy ceramic nanofibers are also added, and the mass ratio of the rare earth high entropy ceramic nanofibers to the magnesium aluminum spinel nanopowder is 1: (1-2) (for example, 1: 1, 1: 1.5 or 1: 2), that is, step (1) is: using water to evenly disperse the high aspect ratio nanofibers, rare earth high entropy ceramic nanofibers, magnesium aluminum spinel nanopowder and nano silicon carbide to obtain a dispersed slurry; in the present invention, when the dispersed slurry contains rare earth high entropy ceramic nanofibers, preferably, the dispersed slurry contains the high aspect ratio nanofibers. The sum of the mass percentages of nanofibers with a diameter ratio, rare earth high entropy ceramic nanofibers and magnesium aluminum spinel nanopowder is 10-20%; in the present invention, preferably, the dispersed slurry also contains rare earth high entropy ceramic nanofibers. The present invention finds that introducing it into the nano thermal insulation material can effectively improve the overall strength of the material, making it stronger and more durable when subjected to external pressure and mechanical stress, and can increase the multiple scattering and reflection effects of thermal radiation, thereby improving the thermal insulation performance, and can further enhance the mechanical properties and thermal insulation properties of the multi-dimensionally assembled nano thermal insulation material.

[0035] According to some preferred embodiments, the aspect ratio (average aspect ratio) of the rare earth high entropy ceramic nanofiber is (50-100):1. Different from the high aspect ratio nanofibers used as the main raw material of the nanofiber thermal insulation skeleton, the present invention preferably uses rare earth high entropy ceramic nanofibers with an aspect ratio of (50-100):1. The present invention finds that two nanofibers with different aspect ratios can form a multi-scale enhancement effect. The rare earth high entropy ceramic nanofibers with a smaller aspect ratio can fill the gaps between the high aspect ratio nanofibers to form a more compact and uniform structure. This multi-scale structure can more effectively transmit and disperse stress and improve the overall mechanical properties of the material. The mixture of two nanofibers with different aspect ratios can form a pore structure with different sizes and shapes, optimize the pore structure, and this multi-scale pore structure can effectively block the heat conduction path and reduce the heat conduction efficiency, thereby improving the thermal insulation performance of the material. The present invention is more preferably to add rare earth high entropy ceramic nanofibers with an aspect ratio of (50-100):1, which can effectively improve the mechanical properties and thermal insulation properties of the nano thermal insulation material.

[0036] According to some preferred embodiments, the rare earth high entropy ceramic nanofibers are rare earth zirconate high entropy ceramic nanofibers A2Zr2O7 and / or rare earth hafnium salt high entropy ceramic nanofibers B2Hf2O7; A is any five of the rare earth elements La (lanthanum), Sr (strontium), Ce (cerium), Er (erbium), Y (yttrium) and Yb (ytterbium), and the sum of the atomic molar percentages of each rare earth element is 100%, and the atomic molar percentages of each rare earth element are equal, or the atomic molar percentages differ by no more than 1 to 3%; B is any five of the rare earth elements Nd (neodymium), Sm (samarium), Eu (europium), Gd (gadolinium), Dy (dysprosium) and Er (erbium), and the sum of the atomic molar percentages of each rare earth element is 100%, and the atomic molar percentages of each rare earth element are equal, or the atomic molar percentages differ by no more than 1 to 3%.

[0037] According to some more preferred embodiments, the rare earth high entropy ceramic nanofiber is (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic nanofibers, (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Y 0.2 )2Zr2O7 high entropy ceramic nanofibers, (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic nanofibers or (Nd 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high-entropy ceramic nanofibers; the present invention finds that these high-entropy ceramic nanofibers can outperform other high-entropy ceramic nanofibers in many aspects such as high-temperature stability, thermal conductivity, and optical reflection performance, thereby preparing a multi-dimensionally assembled nano-insulation material with even better performance. The reasonable combination of rare earth elements can provide a variety of favorable physical and chemical properties, such as excellent optical properties, thermal stability and chemical stability. The reasonable combination of these elements has a significant effect on improving the comprehensive performance of the material. Due to the reasonable combination of rare earth elements in these high-entropy ceramic nanofibers, the material has a lower thermal conductivity and can effectively block heat conduction, which is more conducive to improving the thermal insulation performance of the nano-insulation material.

[0038] The present invention does not specifically limit the source of rare earth zirconate high entropy ceramic nanofibers A2Zr2O7 and / or rare earth hafniumate high entropy ceramic nanofibers B2Hf2O7, for example, they can be directly purchased products or products prepared by existing methods; in the present invention, specifically, (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic nanofibers as an example, the preparation steps may be:

[0039] ① Prepared by sol-gel method (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic dispersion: wherein lanthanum acetate, strontium acetate, cerium acetate, erbium acetate, ytterbium acetate, basic zirconium carbonate are used as raw materials, and acetic acid aqueous solution is used as solvent; according to (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 The raw materials were added into an acetic acid aqueous solution (the mass ratio of acetic acid to water was 1:1) and stirred for 0.5h to obtain (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic dispersion, making (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 ) The solid content (concentration) of the 2Zr2O7 high entropy ceramic dispersion is 15wt%;

[0040] ② Add polyethylene oxide to the (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic dispersion, stirring evenly to prepare a spinning solution, so that the mass percentage of polyethylene oxide in the spinning solution is 2%;

[0041] ③ The prepared spinning solution was sucked into the syringe of the electrospinning equipment, and the electrospinning parameters were set, including a voltage of 20 kV, a push speed of 0.4 mm / min, and a distance of 15 cm. After setting the parameters, the spinning solution was electrospun, then dried in a blast drying oven at 70 ° C for 12 hours, and then calcined in an air atmosphere at 1200 ° C for 2 hours to obtain (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic nanofibers.

[0042] In the present invention, to prepare (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic nanofibers as an example, the preparation steps may be:

[0043] ① Prepared by sol-gel method (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic dispersion: wherein samarium acetate, europium acetate, gadolinium acetate, dysprosium acetate, erbium acetate, and hafnium chloride are used as raw materials, and acetic acid aqueous solution is used as solvent; according to (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 The raw materials were added into an acetic acid aqueous solution (the mass ratio of acetic acid to water was 1:1) and stirred for 0.5 h to obtain (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic dispersion, making (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 ) The solid content (concentration) of the 2Hf2O7 high entropy ceramic dispersion is 15wt%;

[0044] ② Add polyethylene oxide to the (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2)2Hf2O7 high entropy ceramic dispersion, stirring evenly to prepare a spinning solution, so that the mass percentage of polyethylene oxide in the spinning solution is 2%;

[0045] ③ The prepared spinning solution was sucked into the syringe of the electrospinning equipment, and the electrospinning parameters were set, including a voltage of 20 kV, a push speed of 0.4 mm / min, and a distance of 15 cm. After setting the parameters, the spinning solution was electrospun, and then dried in a blast drying oven at 70 ° C for 12 hours. After calcination at a high temperature of 1200 ° C in air atmosphere for 2 hours, (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic nanofibers.

[0046] In a second aspect, the present invention provides a multi-dimensionally assembled nano thermal insulation material prepared by the preparation method described in the first aspect of the present invention.

[0047] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.

[0048] Example 1

[0049] (1) Alumina nanofibers with an aspect ratio of 200:1, magnesium aluminum spinel nanopowder with a particle size of 20 nm, and nano silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of the alumina nanofibers to the magnesium aluminum spinel nanopowder is 9:1, and the mass of the nano silicon carbide is 5% of the sum of the masses of the alumina nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the alumina nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 10%.

[0050] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 90° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 5% of the mass amount of alumina nanofibers in step (1).

[0051] (3) The wet gel obtained in step (2) is placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol is 1:2) and the solvent is replaced three times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 48 hours to obtain a multi-dimensionally assembled nano thermal insulation material.

[0052] Example 2

[0053] (1) Alumina nanofibers with an aspect ratio of 1000:1, magnesium aluminum spinel nanopowder with a particle size of 200 nm, and nano silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of the alumina nanofibers to the magnesium aluminum spinel nanopowder is 1:1, and the mass of the nano silicon carbide is 5% of the sum of the mass of the alumina nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the alumina nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 20%.

[0054] (2) Add calcium aluminate cement to the dispersed slurry obtained in step (1), stir and disperse evenly, and then age at 60° C. for 24 hours to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 15% of the mass amount of alumina nanofibers in step (1).

[0055] (3) The wet gel obtained in step (2) is placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol is 1:2) and the solvent is replaced 5 times, each solvent replacement time is 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 72 hours to obtain a multi-dimensional assembled nano thermal insulation material.

[0056] Example 3

[0057] (1) Place zirconium oxide nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel nanopowder with a particle size of 50 nm, and nano silicon carbide with a particle size of 50 nm in water, stir and disperse them, and obtain a dispersed slurry; wherein the mass ratio of zirconium oxide nanofibers to magnesium aluminum spinel nanopowder is 4:1, and the mass of nano silicon carbide is 5% of the sum of the mass of zirconium oxide nanofibers and magnesium aluminum spinel nanopowder; and the sum of the mass percentages of zirconium oxide nanofibers and magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0058] (2) adding a zirconium oxide-calcium phosphate composite sol gelling agent to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 hours to obtain a wet gel; in step (2), the mass amount of the zirconium oxide-calcium phosphate composite sol gelling agent is 20% of the mass amount of the zirconium oxide nanofibers in step (1).

[0059] (3) The wet gel obtained in step (2) is placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol is 1:2) and the solvent is replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a multi-dimensional assembled nano thermal insulation material.

[0060] Example 4

[0061] (1) Place zirconium silicate nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel nanopowder with a particle size of 50 nm, and nano silicon carbide with a particle size of 50 nm in water, stir and disperse them, and obtain a dispersed slurry; wherein the mass ratio of the zirconium silicate nanofibers to the magnesium aluminum spinel nanopowder is 4:1, and the mass of the nano silicon carbide is 5% of the sum of the mass of the zirconium silicate nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the zirconium silicate nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0062] (2) adding calcium aluminosilicate cement to the dispersed slurry obtained in step (1), stirring and dispersing, and then aging at 80° C. for 48 hours to obtain a wet gel; in step (2), the mass amount of calcium aluminosilicate cement is 20% of the mass amount of zirconium silicate nanofibers in step (1).

[0063] (3) The wet gel obtained in step (2) was placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol was 1:2) for solvent replacement 4 times, each solvent replacement time was 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a multi-dimensionally assembled nano thermal insulation material.

[0064] Example 5

[0065] (1) Mullite nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel nanopowders with a particle size of 50 nm, and nano-silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed, and a dispersed slurry is obtained; wherein the mass ratio of the mullite nanofibers to the magnesium aluminum spinel nanopowder is 4:1, and the mass of the nano-silicon carbide is 5% of the sum of the mass of the mullite nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the mullite nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0066] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 20% of the mass amount of mullite nanofibers in step (1).

[0067] (3) The wet gel obtained in step (2) is placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol is 1:2) and the solvent is replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a multi-dimensional assembled nano thermal insulation material.

[0068] Example 6

[0069] (1) Magnesium aluminum spinel nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel nanopowders with a particle size of 50 nm, and nano silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of magnesium aluminum spinel nanofibers to magnesium aluminum spinel nanopowders is 4:1, the mass of silicon carbide is 5% of the sum of the mass of magnesium aluminum spinel nanofibers and magnesium aluminum spinel nanopowders; and the sum of the mass percentages of magnesium aluminum spinel nanofibers and magnesium aluminum spinel nanopowders in the dispersed slurry is 15%.

[0070] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing, and then aging at 80° C. for 48 hours to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 20% of the mass amount of magnesium aluminate spinel nanofibers in step (1).

[0071] (3) The wet gel obtained in step (2) is placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol is 1:2) and the solvent is replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a multi-dimensional assembled nano thermal insulation material.

[0072] Example 7

[0073] Example 7 is substantially the same as Example 5, except that:

[0074] (1) Mullite nanofibers with an aspect ratio of 2000:1 and (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 )2Zr2O7 high entropy ceramic nanofibers, magnesium aluminum spinel nanopowder with a particle size of 50nm and nano silicon carbide with a particle size of 50nm are placed in water and stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of mullite nanofibers to magnesium aluminum spinel nanopowder is 4:1, (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2 The mass ratio of 2Zr2O7 high entropy ceramic nanofibers to magnesium aluminum spinel nanopowders is 1:1.5, and the mass of nano-silicon carbide is 5% of the sum of the mass of mullite nanofibers (nanofibers with high aspect ratio) and magnesium aluminum spinel nanopowders; the dispersed slurry contains mullite nanofibers, (La 0.2 Sr 0.2 Ce 0.2 Er 0.2 Yb 0.2The sum of the mass percentages of 2Zr2O7 high entropy ceramic nanofibers and magnesia alumina spinel nanopowder is 15%.

[0075] Example 8

[0076] Embodiment 8 is substantially the same as Embodiment 5, except that:

[0077] (1) Mullite nanofibers with an aspect ratio of 2000:1 and (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 )2Hf2O7 high entropy ceramic nanofibers, magnesium aluminum spinel nanopowder with a particle size of 50nm and nano silicon carbide with a particle size of 50nm are placed in water and stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of mullite nanofibers to magnesium aluminum spinel nanopowder is 4:1, (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 The mass ratio of )2Hf2O7 high entropy ceramic nanofibers to magnesium aluminum spinel nanopowders is 1:1.5, and the mass of nano silicon carbide is 5% of the sum of the mass of mullite nanofibers (nanofibers with high aspect ratio) and magnesium aluminum spinel nanopowders; the dispersed slurry contains mullite nanofibers, (Sm 0.2 Eu 0.2 G 0.2 Dy 0.2 Er 0.2 The sum of the mass percentages of 2Hf2O7 high entropy ceramic nanofibers and magnesia alumina spinel nanopowder is 15%.

[0078] Example 9

[0079] Example 9 is substantially the same as Example 5, except that:

[0080] (3) The wet gel obtained in step (2) is placed in ethanol for solvent replacement 4 times, each solvent replacement time is 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a multi-dimensionally assembled nano thermal insulation material.

[0081] Comparative Example 1

[0082] Comparative Example 1 is substantially the same as Example 5, except that:

[0083] (1) Mullite nanofibers with an aspect ratio of 50:1, magnesium aluminum spinel nanopowders with a particle size of 50 nm, and nano-silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed, and a dispersed slurry is obtained; wherein the mass ratio of the mullite nanofibers to the magnesium aluminum spinel nanopowder is 4:1, the mass of the nano-silicon carbide is 5% of the sum of the mass of the mullite nanofibers and the magnesium aluminum spinel nanopowder, and the sum of the mass percentages of the mullite nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0084] The aspect ratio of the mullite nanofiber used in this comparative example is too small, and it is difficult to form a skeleton structure during the preparation process, and the nano thermal insulation material cannot be obtained.

[0085] Comparative Example 2

[0086] (1) Mullite nanofibers with an aspect ratio of 20000:1, magnesium aluminum spinel nanopowders with a particle size of 50 nm, and nano-silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed, and a dispersed slurry is obtained; wherein the mass ratio of the mullite nanofibers to the magnesium aluminum spinel nanopowder is 4:1, and the mass of the nano-silicon carbide is 5% of the sum of the mass of the mullite nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the mullite nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0087] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 20% of the mass amount of mullite nanofibers in step (1).

[0088] (3) The wet gel obtained in step (2) was placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol was 1:2) and the solvent was replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a nano thermal insulation material.

[0089] Comparative Example 3

[0090] (1) Mullite nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel nanopowders with a particle size of 50 nm, and nano silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed, and a dispersed slurry is obtained; wherein the mass ratio of the mullite nanofibers to the magnesium aluminum spinel nanopowder is 4:1, and the mass of silicon carbide is 5% of the sum of the mass of the mullite nanofibers and the magnesium aluminum spinel nanopowder; and the sum of the mass percentages of the mullite nanofibers and the magnesium aluminum spinel nanopowder in the dispersed slurry is 15%.

[0091] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 41.67% of the mass amount of mullite nanofibers in step (1).

[0092] (3) The wet gel obtained in step (2) was placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol was 1:2) and the solvent was replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a nano thermal insulation material.

[0093] Comparative Example 4

[0094] (1) Mullite nanofibers with an aspect ratio of 2000:1, magnesium aluminum spinel powder with a particle size of 5 μm, and nano-silicon carbide with a particle size of 50 nm are placed in water and stirred and dispersed to obtain a dispersed slurry; wherein the mass ratio of mullite nanofibers to magnesium aluminum spinel powder is 4:1, and the mass of nano-silicon carbide is 5% of the sum of the mass of mullite nanofibers and magnesium aluminum spinel powder; and the sum of the mass percentages of mullite nanofibers and magnesium aluminum spinel powder in the dispersed slurry is 15%.

[0095] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 20% of the mass amount of mullite nanofibers in step (1).

[0096] (3) The wet gel obtained in step (2) was placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol was 1:2) and the solvent was replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a nano thermal insulation material.

[0097] Comparative Example 5

[0098] (1) Mullite nanofibers with an aspect ratio of 2000:1 and nano-silicon carbide with a particle size of 50 nm are placed in water, stirred and dispersed to obtain a dispersed slurry; wherein the mass of the nano-silicon carbide is 5% of the mass of the mullite nanofibers, and the mass percentage of the mullite nanofibers in the dispersed slurry is 15%.

[0099] (2) adding calcium aluminate cement to the dispersed slurry obtained in step (1), stirring and dispersing the slurry uniformly, and subjecting the slurry to high temperature aging at 80° C. for 48 h to obtain a wet gel; in step (2), the mass amount of calcium aluminate cement is 20% of the mass amount of mullite nanofibers in step (1).

[0100] (3) The wet gel obtained in step (2) was placed in a cyclohexane / ethanol mixed solvent (the volume ratio of cyclohexane to ethanol was 1:2) and the solvent was replaced 4 times, each time for 24 hours, and then sent to a supercritical drying kettle for supercritical carbon dioxide drying for 96 hours to obtain a nano thermal insulation material.

[0101] Comparative Example 6

[0102] Comparative Example 6 is substantially the same as Example 5, except that:

[0103] (2) adding silica sol (solid content of silica sol is 30 wt%) and polyethylene oxide (PEO) to the dispersed slurry obtained in step (1), stirring and dispersing to obtain a mixed solution; wherein the mass amount of silica sol is 10% of the mass amount of the mullite nanofibers in step (1), and the mass amount of polyethylene oxide is 2% of the mass amount of the mullite nanofibers in step (1).

[0104] (3) The mixed solution was rapidly frozen with liquid nitrogen for 30 minutes, and finally freeze-dried at -10°C for 72 hours and calcined at 600°C for 2 hours to obtain a nano thermal insulation material.

[0105] Comparative Example 7

[0106] Comparative Example 7 is substantially the same as Example 5, except that:

[0107] (2) adding an aqueous solution of aluminum dihydrogen phosphate (the solid content of the aqueous solution of aluminum dihydrogen phosphate is 40 wt%) and polyethylene oxide (PEO) to the dispersed slurry obtained in step (1), stirring and dispersing to obtain a mixed solution; wherein the mass amount of the aqueous solution of aluminum dihydrogen phosphate is 10% of the mass amount of the mullite nanofibers in step (1), and the mass amount of polyethylene oxide is 2% of the mass amount of the mullite nanofibers in step (1).

[0108] (3) The mixed solution was rapidly frozen with liquid nitrogen for 30 minutes, and finally freeze-dried at -10°C for 72 hours and calcined at 600°C for 2 hours to obtain a nano thermal insulation material.

[0109] The thermal conductivity and compressive strength at a deformation of 10% of the materials prepared in the embodiments of the present invention and the comparative examples were measured, and the results are shown in Table 1. It can be seen from Table 1 that the materials prepared in the preferred embodiments of the present invention have low thermal conductivity and high compressive strength at high temperatures.

[0110] Table 1

[0111]

[0112]

[0113] In Table 1, the symbol “-” indicates that the performance indicator does not exist.

[0114] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a multi-dimensionally assembled nano thermal insulation material, characterized in that: The method comprises the following steps: (1) using water to uniformly disperse nanofibers with a high aspect ratio, magnesium aluminum spinel nanopowder, and nano silicon carbide to obtain a dispersed slurry; (2) adding a high temperature adhesive to the dispersed slurry and dispersing it uniformly, and then aging it to obtain a wet gel; the high temperature adhesive is one or more of a calcium aluminate cement gelling agent, a zirconium oxide-calcium phosphate composite sol gelling agent, and a calcium aluminosilicate cement gelling agent; (3) The wet gel is subjected to solvent replacement and supercritical drying in sequence to obtain a multi-dimensionally assembled nano thermal insulation material.

2. The preparation method according to claim 1, characterized in that: The nanofibers are one or more of zirconium oxide nanofibers, magnesium aluminum spinel nanofibers, zirconium silicate nanofibers, mullite nanofibers and aluminum oxide nanofibers.

3. The preparation method according to claim 1, characterized in that: The aspect ratio of the nanofiber is (200-10000):1; and / or The particle size of the magnesium aluminum spinel nanopowder is 20nm-200nm.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the nanofiber to the magnesium aluminum spinel nanopowder is (1-9):1; and / or The mass dosage of the nano silicon carbide is 4-8% of the sum of the mass dosages of the nano fiber and the magnesium aluminum spinel nano powder.

5. The preparation method according to claim 1, characterized in that: The sum of the mass percentages of the nanofibers and the magnesium aluminum spinel nanopowder contained in the dispersed slurry is 10-20%; and / or The mass amount of the high temperature adhesive in step (2) is 5 to 20% of the mass amount of the nanofibers in step (1).

6. The preparation method according to claim 1, characterized in that: The aging temperature is 60° C. to 90° C., and the aging time is 12 h to 48 h.

7. The preparation method according to claim 1, characterized in that: The number of solvent replacements is 3 to 5 times; The solvent replacement uses a cyclohexane / ethanol mixed solvent as the solvent, preferably, the cyclohexane / ethanol mixed solvent is a mixture of n-hexane and ethanol in a volume ratio of 1: (1-3); and / or The supercritical drying time is 48 to 96 hours.

8. The preparation method according to claim 1, characterized in that: In step (1), rare earth high entropy ceramic nanofibers are also added, and the mass ratio of the rare earth high entropy ceramic nanofibers to the magnesium aluminum spinel nanopowder is 1: (1-2).

9. The preparation method according to claim 8, characterized in that: The rare earth high entropy ceramic nanofibers are rare earth zirconate high entropy ceramic nanofibers A2Zr2O7 and / or rare earth hafniumate high entropy ceramic nanofibers B2Hf2O7; A is any five of the rare earth elements La, Sr, Ce, Er, Y and Yb, and the sum of the atomic mole percentages of the rare earth elements is 100%, and the atomic mole percentages of the rare earth elements are equal, or the atomic mole percentages differ by no more than 1 to 3%; B is any five of the rare earth elements Nd, Sm, Eu, Gd, Dy and Er, and the sum of the atomic mole percentages of the rare earth elements is 100%, and the atomic mole percentages of the rare earth elements are equal, or the atomic mole percentages differ by no more than 1 to 3%.

10. The multi-dimensionally assembled nano thermal insulation material prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of nanowire / silicon-aluminum aerogel composite material

    CN111807810A

  • Alumina fiber magnesium aluminate spinel porous ceramic and preparation method thereof

    CN112279637A

  • Rare-earth-based heat-insulation porous high-entropy ceramic and preparation method thereof

    CN113929453A

  • Nanofiber aerogel composite material with ultralow thermal conductivity and preparation method thereof

    CN114524638A

  • Zirconic acid rare earth-based high-entropy ceramic nanofiber as well as preparation method and application thereof

    CN114751737A