Antibacterial ceramic material and preparation method thereof

By using inorganic calcium compounds as carriers in ceramic materials to form microporous structures, the problem of insufficient antibacterial properties of ceramic materials is solved, and the sustained release and long-term antibacterial effects of antibacterial agents are achieved.

CN118894737AActive Publication Date: 2024-11-05JINDA NAMI TECH XIAMEN CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410951139.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The antibacterial properties of existing ceramic materials are insufficient, mainly due to the strong or weak binding force of the inorganic antibacterial agent and the carrier, which makes the antibacterial agent unable to effectively detach and release, and the antibacterial duration is short.

Method used

Inorganic calcium compounds are used as carriers for antibacterial components, and the slow release and continuous action of the antibacterial agent is ensured by adding antibacterial agents to the glaze or ceramic base material and forming micropores during the sintering process.

Benefits of technology

The long-term antibacterial properties of ceramic materials are achieved, and the antibacterial agent can be released for more than 6 months, providing continuous antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947276880000101
    Figure BDA0004947276880000101
  • Figure BDA0004947276880000111
    Figure BDA0004947276880000111
Patent Text Reader

Abstract

The invention provides an antibacterial ceramic material and a preparation method thereof, and relates to the technical field of antibacterial materials. The antibacterial ceramic material consists of a ceramic inner layer and an antibacterial outer layer, the antibacterial outer layer is coated on the outer surface of the ceramic inner layer and contains an antibacterial agent; the antibacterial agent is formed by loading an inorganic antibacterial component on an inorganic carrier, and the inorganic carrier contains an inorganic calcium compound. The antibacterial ceramic material disclosed by the invention has the characteristics of good antibacterial property and lasting antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of antibacterial materials and relates to an antibacterial ceramic material and a preparation method thereof. Background Art

[0002] Ceramics is a traditional building material, which is widely used in various fields due to its advantages such as high strength, wear resistance and corrosion resistance. However, ceramic materials also have some disadvantages, such as easy breeding of bacteria, which will affect its use effect and service life. One solution is to coat the ceramic surface with a glaze layer or ceramic layer with antibacterial properties, such as adding an inorganic antibacterial agent (nanosilver, nanozinc oxide, etc.) to the glaze or ceramic base material and mixing evenly, coating it on the ceramic surface and sintering it to form an antibacterial glaze layer or antibacterial ceramic layer on the ceramic surface.

[0003] However, the antibacterial properties of the antibacterial ceramics obtained by the above method are still insufficient, which is mainly reflected in the following two aspects: (1) the antibacterial rate is poor; (2) the antibacterial duration is short.

[0004] Therefore, the above problems need to be solved urgently. Summary of the invention

[0005] For the inorganic antibacterial agent in the glaze layer or ceramic layer to work, two steps are required. The first step is that the inorganic antibacterial agent is separated from the carrier, and the second step is that the separated inorganic antibacterial agent passes through the surface glaze layer or ceramic layer and is released into the environment. The inventors found that the main reasons for the poor antibacterial performance of antibacterial ceramics in the prior art are the following two points: (1) The inorganic antibacterial agent is generally loaded on the carrier first, and the binding force between the inorganic antibacterial agent and the carrier is too good, resulting in the inorganic antibacterial agent being unable to effectively separate from the carrier, or the binding force between the inorganic antibacterial agent and the carrier is too poor, resulting in the inorganic antibacterial agent quickly separating from the carrier completely, and the antibacterial persistence is poor; (2) The glaze layer or ceramic layer after sintering is relatively dense. Even if the inorganic antibacterial agent can separate from the carrier, it cannot penetrate the dense glaze layer or ceramic layer and be released into the environment, resulting in insufficient antibacterial performance. Surprisingly, the use of inorganic calcium compounds as carriers of antibacterial components can solve the above problems. Based on this, the present invention provides an antibacterial ceramic material and a preparation method thereof.

[0006] The technical solution of the present invention is as follows:

[0007] An antibacterial ceramic material, consisting of ceramic and an antibacterial outer layer;

[0008] The antibacterial outer layer is coated on the outer surface of the ceramic, and the antibacterial outer layer contains an antibacterial agent;

[0009] The antibacterial agent is an inorganic antibacterial component loaded on an inorganic carrier;

[0010] The inorganic carrier comprises an inorganic calcium compound.

[0011] Preferably, the weight proportion of the antibacterial agent in the antibacterial outer layer is not higher than 20% and not lower than 3%.

[0012] Preferably, the inorganic antibacterial component is selected from one or a combination of two or more of silver antibacterial agent and nano zinc oxide.

[0013] More preferably, the silver antibacterial agent is selected from one or a combination of two or more of nano silver particles, silver nitrate, nano silver oxide particles, silver sulfate, silver phosphate and silver ammonium phosphate.

[0014] More preferably, the inorganic antibacterial component consists of silver antibacterial agent and nano zinc oxide in a weight ratio of 1:20-1:1.

[0015] Preferably, the weight ratio of the inorganic antibacterial component to the inorganic carrier is 3-20:80-97.

[0016] Preferably, the inorganic calcium compound is selected from one or a combination of two or more of calcium oxide, calcium carbonate, calcium hydroxide, calcium sulfate, calcium chloride, dicalcium hydrogen phosphate and calcium phosphate.

[0017] Preferably, the inorganic carrier further comprises a second carrier, the weight proportion of the second carrier in the inorganic carrier is not higher than 30%, and the second carrier is selected from one or a combination of two or more of zirconium phosphate, silica, zeolite, attapulgite, montmorillonite, bentonite and kaolin.

[0018] Preferably, the preparation method of the antibacterial agent is: mixing and dispersing the inorganic antibacterial component and the inorganic carrier to obtain the antibacterial agent.

[0019] A method for preparing the antibacterial ceramic material according to any one of the above embodiments comprises the following steps:

[0020] S1, adding the antibacterial agent to the glaze base material or the ceramic base material, mixing evenly, and obtaining a premix;

[0021] S2, coating the premixed material in step S1 on the ceramic surface and sintering to obtain the antibacterial ceramic material.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention uses an inorganic calcium compound as a carrier of the inorganic antibacterial component, which has two functions: 1) The inorganic calcium compound has a moderate binding force with the inorganic antibacterial component, and the inorganic antibacterial component can slowly and continuously detach from the inorganic calcium compound and be released; 2) When the antibacterial agent is added to the glaze base material or the ceramic base material and sintered to prepare the antibacterial glaze layer or the antibacterial ceramic layer, tiny openings or more micropores can be formed in the glaze layer or the ceramic layer, which is conducive to the continuous release of the antibacterial components detached from the carrier into the environment through the openings.

[0024] (2) The antibacterial ceramic material of the present invention has a long-lasting antibacterial property and can continuously release inorganic antibacterial components for 6 months or more, thus continuously providing good antibacterial properties. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0026] In order to solve the problems of poor antibacterial properties of existing ceramics, poor antibacterial properties of antibacterial glaze layers, and inability to continuously provide antibacterial properties, on the one hand, the present invention provides an antibacterial ceramic material, which is composed of ceramics and an antibacterial outer layer;

[0027] The antibacterial outer layer is coated on the outer surface of the ceramic, and the antibacterial outer layer contains an antibacterial agent;

[0028] The antimicrobial agent is an inorganic antimicrobial component loaded on an inorganic carrier;

[0029] The inorganic carrier comprises an inorganic calcium compound.

[0030] The antibacterial outer layer may be an antibacterial ceramic layer or an antibacterial glaze layer, that is, the main material of the antibacterial outer layer is ceramic or glaze.

[0031] In the present invention, the antibacterial outer layer contains an antibacterial agent, which is an inorganic antibacterial component loaded on an inorganic carrier. The inorganic carrier can improve the dispersibility of the inorganic antibacterial component, and the inorganic carrier contains at least an inorganic calcium compound, which can have the following two effects: (1) the inorganic calcium compound has a moderate binding force with the inorganic antibacterial component, and the inorganic antibacterial component can gradually detach from the surface of the inorganic calcium compound; (2) the use of the inorganic calcium compound can form micropores or more micropores in the antibacterial outer layer during the sintering process of the antibacterial outer layer, which helps the detached inorganic antibacterial component to penetrate the antibacterial outer layer and be released into the environment, thereby playing an antibacterial role.

[0032] In a preferred embodiment of the present invention, the weight proportion of the antibacterial agent in the antibacterial outer layer is not higher than 20% and not lower than 3%. If the weight proportion of the antibacterial agent in the antibacterial outer layer is too high, the performance of the antibacterial outer layer will be insufficient, such as insufficient adhesion to the ceramic inner layer, or too many micropores, affecting the quality of the antibacterial outer layer, and the antibacterial components are released too quickly; if the weight proportion of the antibacterial agent in the antibacterial outer layer is insufficient, the antibacterial performance of the antibacterial outer layer will be insufficient. For example, the weight proportion of the antibacterial agent in the antibacterial outer layer can be any value of 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc., but not limited to the above. Or, further, the weight proportion of the antibacterial agent in the antibacterial outer layer can be 5%-18%.

[0033] In a preferred embodiment of the present invention, the inorganic antibacterial component is selected from one or a combination of two or more of silver antibacterial agents and nano zinc oxide. In the present invention, the inorganic antibacterial component can be directly obtained from the market or prepared according to the prior art, and the average particle size of the inorganic antibacterial component can be 10nm-100nm. Silver antibacterial agents and nano zinc oxide are both commonly used inorganic antibacterial components with good antibacterial properties. Further, the silver antibacterial agent can be selected from one or a combination of two or more of nano silver particles, silver nitrate, nano silver oxide particles, silver sulfate, silver phosphate and silver ammonium phosphate.

[0034] In a more preferred embodiment of the present invention, the inorganic antibacterial component is composed of a silver antibacterial agent and nano zinc oxide in a weight ratio of 1:20-1:1. The inorganic antibacterial component is composed of a silver antibacterial agent and nano zinc oxide, which can synergistically exert the effects of the two antibacterial agents and further improve the antibacterial performance. For example, the weight ratio of the silver antibacterial agent and nano zinc oxide can be any value in 1:20, 1:19, 1:18, 1:17, 1:16, 1:15, 1:14, 1:13, 1:12, 1:11, 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, etc., but is not limited to the above-listed ones. Further preferably, the inorganic antibacterial component is composed of a silver antibacterial agent and nano zinc oxide in a weight ratio of 1:15-1:3.

[0035] In a preferred embodiment of the present invention, the weight ratio of the inorganic antibacterial component to the inorganic carrier is 3-20:80-97. In the present invention, the average particle size of the inorganic carrier can be 200nm-5μm. When the weight ratio of the inorganic antibacterial component to the inorganic carrier is within the above range, a better loading effect can be obtained. If the inorganic carrier is less and the inorganic antibacterial component is more, some of the inorganic antibacterial components will be unevenly dispersed and agglomerated. If the inorganic carrier is too much and the inorganic antibacterial component is less, the utilization rate of the inorganic carrier will be insufficient, and the antibacterial agent will be less, affecting the antibacterial performance. For example, the weight ratio of the inorganic antibacterial component to the inorganic carrier can be any value in 3:97, 4:96, 5:95, 6:94, 7:93, 8:92, 9:91, 10:90, 11:89, 12:88, 13:87, 14:86, 15:85, 16:84, 17:83, 18:82, 19:81, 20:80, etc., but not limited to the above. Alternatively, further, the weight ratio of the inorganic antibacterial component to the inorganic carrier can be 5-17:83-95.

[0036] In a preferred embodiment of the present invention, the inorganic calcium compound is selected from one or a combination of two or more of calcium oxide, calcium carbonate, calcium hydroxide, calcium sulfate, calcium chloride, dicalcium phosphate and calcium phosphate. The above inorganic calcium compound is used as an inorganic carrier or one of the inorganic carriers, and the binding force with the inorganic antibacterial component is moderate, and the speed at which the inorganic antibacterial component detaches from the inorganic carrier is moderate, not too fast or too slow. If the detachment is too fast, it is impossible to achieve a long-term continuous antibacterial property. If the detachment is too slow, less inorganic antibacterial components are released, and the antibacterial property will be insufficient.

[0037] In a preferred embodiment of the present invention, the inorganic carrier further comprises a second carrier, the weight proportion of the second carrier in the inorganic carrier is not higher than 30%, and the second carrier can be selected from one or a combination of two or more of zirconium phosphate, silica, zeolite, attapulgite, montmorillonite, bentonite and kaolin. The inorganic carrier of the present invention, in addition to containing an inorganic calcium compound, can also contain a second carrier, and the second carrier has a good binding force with the inorganic antibacterial component, such as the inorganic antibacterial component and the inorganic calcium compound have a higher binding force, which will inhibit the detachment speed of the inorganic antibacterial component. Therefore, the weight proportion of the second carrier in the inorganic carrier cannot be too high, which will affect the detachment speed of the inorganic antibacterial component and further affect the antibacterial performance. Further preferably, the weight proportion of the second carrier in the inorganic carrier may be not less than 3%. For example, the weight proportion of the second carrier in the inorganic carrier may be any value among 3%, 5%, 7%, 9%, 10%, 12%, 14%, 15%, 17%, 20%, 22%, 23%, 25%, 27%, 28%, 30%, etc., but not limited to the above. Adding the second carrier can inhibit the excessive release of the inorganic antibacterial component in the early stage, which is conducive to maintaining a more stable release of the inorganic antibacterial component and improving the durability of the release.

[0038] In a preferred embodiment of the present invention, the preparation method of the antibacterial agent is: mixing and dispersing the inorganic antibacterial component and the inorganic carrier. After the inorganic antibacterial component and the inorganic carrier are mixed, the antibacterial agent can be obtained by high-speed dispersion or the like. For example, the speed of high-speed dispersion can be 1200-2000 rpm, and the dispersion time is not specifically limited and can be 2-10 min.

[0039] In another aspect, the present invention provides a method for preparing the antibacterial ceramic material according to any one of the above embodiments, comprising the following steps:

[0040] S1. Add the antibacterial agent to the glaze base material or the ceramic base material, mix well, and obtain a premix;

[0041] S2, coating the premix of step S1 on the ceramic surface and sintering to obtain the antibacterial ceramic material of the present invention.

[0042] The glaze base material or ceramic base material in the above step S1 is not particularly limited and can be a commercially available product, or prepared by referring to the formula composition and preparation method in the prior art CN116854373B, CN116282921B, CN116177985B, CN115974411B, etc.

[0043] In the above step S2, there is no particular restriction on the coating thickness of the premix on the ceramic surface. Taking the antibacterial outer layer as an antibacterial glaze layer as an example, the thickness of the antibacterial outer layer on the surface of the sintered antibacterial ceramic material can be 0.1-2 mm, the sintering temperature can be 500-800°C, and the sintering time can be 1.5-3 hours.

[0044] The technical scheme of the present invention is further described and illustrated below according to various preparation examples and embodiments. Unless otherwise specified, the parts described in the following embodiments are parts by weight.

[0045] Preparation Example 1-10 Preparation of antibacterial agent

[0046] Preparation Example 1

[0047] The inorganic antibacterial component is composed of silver phosphate and nano zinc oxide in a weight ratio of 1:15, and the average particle size is 45nm.

[0048] 5 parts of inorganic antibacterial components and 95 parts of calcium carbonate (average particle size of 2 μm) were mixed and dispersed for 5 minutes under high-speed stirring at 1500 rpm to obtain an antibacterial agent.

[0049] Preparation Example 2

[0050] The difference between Preparation Example 2 and Preparation Example 1 is that in Preparation Example 1, the weight ratio of silver phosphate to nano zinc oxide is adjusted from 1:15 to 1:10. The other steps remain unchanged.

[0051] Preparation Example 3

[0052] The difference between Preparation Example 3 and Preparation Example 1 is that in Preparation Example 1, the weight ratio of silver phosphate to nano zinc oxide is adjusted from 1:15 to 1:4. The other steps remain unchanged.

[0053] Preparation Example 4

[0054] The difference between Preparation Example 4 and Preparation Example 3 is that in Preparation Example 3, the inorganic antibacterial agent is adjusted from 5 parts to 12 parts, and the calcium carbonate is adjusted from 95 parts to 88 parts. The other steps remain unchanged.

[0055] Preparation Example 5

[0056] The difference between Preparation Example 5 and Preparation Example 3 is that in Preparation Example 3, the inorganic antibacterial agent is adjusted from 5 parts to 20 parts, and the calcium carbonate is adjusted from 95 parts to 80 parts. The other steps remain unchanged.

[0057] Preparation Example 6

[0058] The difference between Preparation Example 6 and Preparation Example 3 is that in Preparation Example 3, all the inorganic antibacterial components are adjusted to silver phosphate. The other steps remain unchanged.

[0059] Preparation Example 7

[0060] The difference between Preparation Example 7 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to an equal weight of calcium sulfate (average particle size 2 μm). The remaining steps remain unchanged.

[0061] Preparation Example 8

[0062] The difference between Preparation Example 8 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to a combination of calcium carbonate and zirconium phosphate (average particle size 2 μm) in a weight ratio of 20:1. The remaining steps remain unchanged.

[0063] Preparation Example 9

[0064] The difference between Preparation Example 9 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to a combination of calcium carbonate and zirconium phosphate (average particle size 2 μm) in a weight ratio of 3:1. The remaining steps remain unchanged.

[0065] Preparation Example 10

[0066] The difference between Preparation Example 10 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to a combination of calcium carbonate and zeolite (average particle size 2 μm) in a weight ratio of 10:1. The remaining steps remain unchanged.

[0067] Comparative Preparation Example 1

[0068] The difference between Preparation Example 1 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to an equal weight of zeolite (average particle size 2 μm), and the remaining steps remain unchanged.

[0069] Comparative Preparation Example 2

[0070] The difference between Preparation Example 2 and Preparation Example 3 is that in Preparation Example 3, calcium carbonate is adjusted to an equal weight of zirconium phosphate (average particle size 2 μm), and the remaining steps remain unchanged.

[0071] Comparative Preparation Example 3

[0072] The difference between the comparative preparation example 3 and the preparation example 3 is that in the preparation example 3, the calcium carbonate is adjusted to an equal weight of mesoporous silica (average particle size 2 μm). The other steps remain unchanged.

[0073] In the following Examples 1-12 and Comparative Examples 1-5, the composition of the glaze base material is: 58 parts of potassium-sodium feldspar, 14 parts of burned talc, 14 parts of Suzhou soil, 3 parts of dolomite, 1.5 parts of zinc oxide, 0.5 parts of barium carbonate, 3 parts of zirconium silicate, and 3 parts of calcium phosphate.

[0074] Example 1

[0075] 100 parts of the above glaze base material were loaded into a ball mill, 90 parts of water were added, ball milled for 10 hours, sieved, 3 parts of the antibacterial agent of Preparation Example 3 were added to the obtained slurry, and stirred at 1200 rpm for 20 minutes to obtain a premix.

[0076] The premix was coated on the surface of ceramic microspheres with an average diameter of 3 mm, dried, and sintered at 650° C. for 2 h to obtain an antibacterial ceramic material with an average thickness of the glaze layer of 1 mm.

[0077] Example 2

[0078] The difference between Example 2 and Example 1 is that in Example 1, the antibacterial agent in Preparation Example 3 is adjusted from 3 parts to 10 parts. The other steps remain unchanged.

[0079] Example 3

[0080] The difference between Example 3 and Example 1 is that in Example 1, the antibacterial agent in Preparation Example 3 is adjusted from 3 parts to 22 parts. The other steps remain unchanged.

[0081] Comparative Example 1

[0082] The difference between Comparative Example 1 and Example 1 is that in Example 1, the antibacterial agent in Preparation Example 3 is adjusted from 3 parts to 30 parts. The other steps remain unchanged.

[0083] Example 4

[0084] The difference between Example 4 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 1. The remaining steps remain unchanged.

[0085] Example 5

[0086] The difference between Example 5 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 2. The remaining steps remain unchanged.

[0087] Example 6

[0088] The difference between Example 6 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 4. The remaining steps remain unchanged.

[0089] Example 7

[0090] The difference between Example 7 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 5. The remaining steps remain unchanged.

[0091] Example 8

[0092] The difference between Example 8 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 6. The remaining steps remain unchanged.

[0093] Example 9

[0094] The difference between Example 9 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 7. The remaining steps remain unchanged.

[0095] Example 10

[0096] The difference between Example 10 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 8. The remaining steps remain unchanged.

[0097] Embodiment 11

[0098] The difference between Example 11 and Example 2 is that in Example 2, the antibacterial agent in Preparation Example 3 is replaced by an equal weight of the antibacterial agent in Preparation Example 9. The remaining steps remain unchanged.

[0099] Example 12

[0100] The difference between Example 12 and Example 2 is that in Example 2, the antibacterial agent of Preparation Example 3 is replaced by an equal weight of the antibacterial agent of Preparation Example 10. The remaining steps remain unchanged.

[0101] Comparative Example 2

[0102] The difference between Comparative Example 2 and Example 2 is that in Example 2, the antibacterial agent of Preparation Example 3 is replaced by an equal weight of the antibacterial agent of Comparative Preparation Example 1. The remaining steps remain unchanged.

[0103] Comparative Example 3

[0104] The difference between Comparative Example 3 and Example 2 is that in Example 2, the antibacterial agent of Preparation Example 3 is replaced by an equal weight of the antibacterial agent of Comparative Preparation Example 2. The remaining steps remain unchanged.

[0105] Comparative Example 4

[0106] The difference between Comparative Example 4 and Example 2 is that in Example 2, the antibacterial agent of Preparation Example 3 is replaced by an equal weight of the antibacterial agent of Comparative Preparation Example 3. The remaining steps remain unchanged.

[0107] Comparative Example 5

[0108] The difference between Comparative Example 5 and Example 2 is that in Example 2, the antibacterial agent of Preparation Example 3 is replaced according to the composition and weight of silver phosphate and nano zinc oxide therein, that is, the antibacterial agent in this comparative example has no carrier, and silver phosphate and nano zinc oxide are directly used. The other steps remain unchanged.

[0109] Antimicrobial agent release test: Take 25g of the antimicrobial ceramic material to be tested and soak it in 4L of water. After soaking for (n-1) days, pour out the solution and add 4L of water to soak for another day. Test the content of the antimicrobial agent in the solution at this time, which is the concentration of the antimicrobial agent ions released by the antimicrobial ceramic material after soaking for the nth day.

[0110] Table 1 below shows the test results of the antibacterial ceramic material of Example 2.

[0111] Table 1

[0112] Number of days <![CDATA[Ag + Concentration / mg / L]]> <![CDATA[Zn 2+ Concentration / mg / L]]> Number of days <![CDATA[Ag + Concentration / mg / L]]> <![CDATA[Zn 2+ Concentration / mg / L]]> 1 0.158 0.742 120 0.051 0.405 7 0.119 0.555 150 0.046 0.388 14 0.078 0.421 180 0.049 0.361 21 0.080 0.479 210 0.041 0.256 30 0.062 0.482 240 0.035 0.248 60 0.050 0.511 300 0.026 0.184 90 0.055 0.549

[0113] It can be seen from the data in Table 1 that the antibacterial ceramic material of the present invention has good antibacterial component release performance.

[0114] The solutions prepared on the 60th, 180th and 240th days were respectively taken and the antibacterial rates of the solutions against Staphylococcus aureus were tested by plate colony counting method, which were 99.9%, 99.9% and 98.5% respectively.

[0115] According to the above-mentioned antimicrobial agent release test method, the antimicrobial component release of the ceramic material to be tested was tested on the first day, 60 days, 120 days and 180 days. The results are shown in Table 2 below.

[0116] Table 2

[0117]

[0118]

[0119] It can be seen from the data in Table 2 that the antibacterial ceramic material of the present invention has good antibacterial sustained-release performance, can continuously release antibacterial components and form a good antibacterial effect. From Comparative Example 1, it can be seen that too much antibacterial agent is added to the glaze, which will greatly increase the cost, but the antibacterial agent release rate is too fast, and the sustained release and sustained antibacterial effects are not good. The antibacterial rate of the solution to Staphylococcus aureus is tested by the plate colony counting method, and the antibacterial rate of the solution on the 120th day does not exceed 80%. From Comparative Examples 2-5, it can be seen that the release of the antibacterial agent is very difficult when zeolite, zirconium phosphate, mesoporous silica, etc. are used as carriers of antibacterial components, and the release amount is very low, and the antibacterial effect is poor. The antibacterial rate of the solution to Staphylococcus aureus is tested by the plate colony counting method. The antibacterial rates of the solutions on the 60th day and 120th day are not more than 50% and not more than 30%, respectively.

[0120] Embodiment 13

[0121] The ceramic base material consists of: 3 parts of quartz sand, 8 parts of potassium-sodium feldspar, 10 parts of ball clay, 17 parts of kaolin, 15 parts of illite clay, 13 parts of pyrophyllite and 2 parts of dolomite.

[0122] The ceramic base material is made into slurry, and then coated on the surface of a ceramic ball with a diameter of 1 cm. After drying, it is sintered at 1250° C. for 2 hours. The thickness of the ceramic outer layer is 2 mm.

[0123] Embodiment 14

[0124] The difference between Example 14 and Example 13 is that the antibacterial agent of Preparation Example 3 is added to the ceramic base material of Example 13, and the antibacterial agent accounts for 8% of the weight of the ceramic base material. The other steps remain unchanged.

[0125] According to the method of GB / T 3810.3-2016 "Test methods for ceramic tiles Part 3: Determination of water absorption, apparent porosity, apparent relative density and bulk density", the apparent porosity of the antibacterial ceramic materials of Examples 13 and 14 was tested respectively. The apparent porosity of the ceramic material of Example 13 was 2.3%, and the apparent porosity of the ceramic material of Example 14 was 3.7%. It can be seen that the addition of an antibacterial agent to the ceramic outer layer in the present invention helps to increase the porosity of the ceramic material, thereby facilitating the release of the antibacterial component.

[0126] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.

Claims

1. An antibacterial ceramic material, It is characterized in that It consists of a ceramic inner layer and an antibacterial outer layer; The antibacterial outer layer is coated on the outer surface of the ceramic inner layer, and the antibacterial outer layer contains an antibacterial agent; The antibacterial agent is an inorganic antibacterial component loaded on an inorganic carrier; The inorganic carrier comprises an inorganic calcium compound.

2. The antibacterial ceramic material according to claim 1, It is characterized in that The weight proportion of the antibacterial agent in the antibacterial outer layer is not higher than 20% and not lower than 3%.

3. The antibacterial ceramic material according to claim 1, It is characterized in that The inorganic antibacterial component is selected from one or a combination of two or more of silver antibacterial agent and nano zinc oxide.

4. The antibacterial ceramic material according to claim 3, It is characterized in that The silver antibacterial agent is selected from one or a combination of two or more of nano silver particles, silver nitrate, nano silver oxide particles, silver sulfate, silver phosphate and silver ammonium phosphate.

5. The antibacterial ceramic material according to claim 3, It is characterized in that The inorganic antibacterial component is composed of a silver antibacterial agent and nano zinc oxide in a weight ratio of 1:20-1:

1.

6. The antibacterial ceramic material according to claim 1, It is characterized in that The weight ratio of the inorganic antibacterial component to the inorganic carrier is 3-20:80-97.

7. The antibacterial ceramic material according to claim 1, It is characterized in that The inorganic calcium compound is selected from one or a combination of two or more of calcium oxide, calcium carbonate, calcium hydroxide, calcium sulfate, calcium chloride, dicalcium hydrogen phosphate and calcium phosphate.

8. The antibacterial ceramic material according to claim 1, It is characterized in that The inorganic carrier also includes a second carrier, the weight proportion of the second carrier in the inorganic carrier is not higher than 30%, and the second carrier is selected from one or a combination of two or more of zirconium phosphate, silica, zeolite, attapulgite, montmorillonite, bentonite and kaolin.

9. The antibacterial ceramic material according to claim 1, It is characterized in that The preparation method of the antibacterial agent is as follows: the inorganic antibacterial component and the inorganic carrier are mixed and dispersed to obtain the antibacterial agent.

10. A method for preparing the antibacterial ceramic material according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1, adding the antibacterial agent to the glaze base material or the ceramic base material, mixing evenly, and obtaining a premix; S2, coating the premixed material in step S1 on the ceramic surface and sintering to obtain the antibacterial ceramic material.

Citation Information

Patent Citations

  • Antibacterial ceramic tile and preparation method thereof

    CN110698227A

  • Nano antibacterial corrosion-resistant ceramic and preparation method thereof

    CN111517830A

  • Anti-agglomeration slow-release inorganic antibacterial material and preparation method thereof

    CN112913856A

  • Novel antibacterial glaze material based on silver nanoclusters

    CN113415994A

  • Ceramic glaze with antibacterial function, and preparation method and application thereof

    CN113860734A