Boron nitride ceramic with low water absorption rate and preparation method thereof
Through boiling and silicon sol impregnation treatment, the water absorption and porosity of boron nitride ceramics are reduced, and the problems of high water absorption and insufficient high-temperature performance of boron nitride ceramics are solved, and efficient dielectric performance and thermal shock resistance are achieved. In aerospace applications.
Patent Information
- Application Number
- CN202411393533.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-10-08
AI Technical Summary
The high water absorption rate of boron nitride ceramics affects its wave transmissive performance, and the performance of existing low-temperature preparation methods may be affected in high temperature or high pressure environments, resulting in material failure.
The first vacuum impregnation of the boron nitride ceramic matrix was used to dry after boiling and drying in the silicon sol, the surface gel was removed, and the porosity was reduced by sintering and the second vacuum impregnation to form a boron nitride ceramic with low water absorption.
It realizes the low water absorption rate, excellent dielectric properties and thermal shock resistance of boron nitride ceramics, and is suitable for the preparation of aerospace wave-transmissive material components, reducing costs and simplifying the process.
Smart Images

Figure CN118894739A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic preparation, and more specifically, relates to a low water absorption boron nitride ceramic and a preparation method thereof. Background Art
[0002] Hexagonal boron nitride (h-BN) ceramics are high-temperature resistant ceramics with great development potential. Its operating temperature exceeds 2800℃ in an inert atmosphere and is as high as 900℃ in oxygen. It has no softening phenomenon at high temperatures, is resistant to strong acid and alkali corrosion, has low thermal expansion coefficient, dielectric constant and loss, and can be used to manufacture high-frequency microwave devices such as filters, resonators, antennas, etc. to protect the normal operation of equipment. It has a wide range of applications in the fields of communication, radar, navigation, etc. However, since boron nitride is a covalent compound with a high melting point, a low solid-phase self-diffusion coefficient, and a lamellar crystal structure, the sintering densification of boron nitride is inhibited, resulting in a certain porosity in boron nitride ceramics. In addition, the raw material powder for preparing boron nitride ceramics often contains hygroscopic boron oxide, which is easy to absorb moisture in an environment with high humidity, affecting the dielectric constant and loss, and then affecting its wave transmission. Therefore, how to seal the pores of boron nitride ceramics without affecting their dielectric properties and strength is one of the problems that need to be solved in the current application of boron nitride ceramics.
[0003] Corresponding improvements have also been made to the above problems. Chinese patent application number CN202410851801.2, published on September 3, 2024, discloses a method for preparing high-density boron nitride ceramic materials at low temperature. Micron-flaky hexagonal boron nitride powder is used as raw material, a small amount of boric acid aqueous solution is added, and the grain structure rearrangement and low-temperature sintering densification of the flaky boron nitride powder are promoted by room temperature pressing and low-temperature pressureless sintering to obtain high-density boron nitride ceramics (density ≥1.90g / cm3). The disadvantage of this patent is that although the preparation process is simple, it may not be able to fully improve its high temperature resistance. When used in high temperature or high pressure environments, the performance of boron nitride ceramics may be seriously affected, and even cause material failure. Summary of the invention
[0004] 1. Problems to be solved In view of the problem that the existing boron nitride ceramics have high water absorption and affect their wave transmission, the present invention provides a low water absorption boron nitride ceramic and a preparation method thereof. The entire preparation process of the present invention is simple, the process is controllable, easy to implement, and is conducive to industrial production. The prepared boron nitride ceramic has high density, low water absorption, excellent dielectric properties and thermal shock resistance, and can be used to prepare aerospace wave-transmitting material components.
[0005] 2. Technical solution To solve the above problems, the present invention adopts the following technical solutions.
[0006] A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: Boil and dry the boron nitride ceramic substrate, and perform the first vacuum impregnation in silica sol; S2: removing the gel on the surface of the boron nitride ceramic substrate after the first vacuum impregnation; S3: sequentially sintering and performing a second vacuum impregnation on the boron nitride ceramic substrate after removing the surface gel; S4: Drying the boron nitride ceramic substrate after the second vacuum impregnation to obtain a boron nitride ceramic with low water absorption.
[0007] By adopting the above technical scheme, the formed boron nitride ceramic matrix is directly boiled, so that the boron oxide in the boron nitride ceramic matrix that is easy to absorb moisture is dissolved and dried in boiling water, thereby reducing the water absorption rate of the boron nitride ceramic matrix to a certain extent; at the same time, the formed boron nitride ceramic matrix itself has a certain low water absorption rate, and can complete the conversion of lower water absorption rate under the premise of having low water absorption rate; then it is placed in silica sol for impregnation, so that the nano silicon dioxide particles in the silica sol are filled into the pores of the boron nitride, thereby reducing the porosity of the boron nitride ceramic matrix; then the silicon hydroxyl groups on the surface of the silicon dioxide that are easy to absorb moisture are removed by sintering, and the porosity of the boron nitride ceramic is further reduced by a second vacuum impregnation, so that the boron nitride has better moisture resistance; the whole process is simple, the process is controllable, and it is easy to implement, which is conducive to industrial production, and the prepared boron nitride ceramic has high density, low water absorption rate, excellent dielectric properties and thermal shock resistance, and can be used to prepare aerospace wave-transparent material components.
[0008] Furthermore, the preparation of the silica sol in step S1 includes dissolving tetraethyl orthosilicate in ethanol and mixing and stirring to obtain a first mixed liquid, adding a second mixed liquid to the first mixed liquid, mixing and stirring, and then standing to obtain silica sol; the second mixed liquid is a mixture of hydrochloric acid and water.
[0009] By adopting the above technical scheme, compared with the traditional method for preparing silica sol, the obtained silica sol particle size is lower, reaching single-digit nanometer-level particle size, while the silica sol prepared by the traditional preparation method is mostly tens of nanometers. Smaller particle size is conducive to fully filling the pores of boron nitride ceramics and effectively reducing the porosity. The silica sol obtained by using tetraethyl orthosilicate as the silicon source has the best performance and a relatively stable process; ethanol is added as a solvent for the hydrolysis of tetraethyl orthosilicate, which will not hinder the hydrolysis and condensation reaction of tetraethyl orthosilicate, and is safer than other alcohols; water is added as a reactant for the hydrolysis of tetraethyl orthosilicate, and hydrochloric acid is added as a hydrolysis catalyst, which can promote the full completion of the hydrolysis reaction and increase the solid content of the silica sol; the mixed solution is configured in the above order, which can make the preparation of silica sol reaction more complete.
[0010] Furthermore, the molar ratio of tetraethyl orthosilicate: ethanol: water: hydrochloric acid is 1:4-20:4-8:1.0×10-3-2.0×10-3; and the pH value is 2-3 after adding the second mixed solution.
[0011] By adopting the above technical scheme, the performance of the silica sol obtained by adding different solvents, reactants, and catalyst concentrations will be greatly different. By setting a suitable molar ratio of tetraethyl orthosilicate, ethanol, water, and hydrochloric acid, the silica sol finally prepared has a smaller particle size and a uniform distribution, and has higher stability, while accelerating the reaction efficiency of the entire preparation process.
[0012] Furthermore, the second mixed liquid is added into the first mixed liquid at a dropping speed of 1 ml / min to 5 ml / min, and the mixing and stirring time after the second mixed liquid is added is 1 h to 5 h.
[0013] By adopting the above technical scheme, by determining a suitable dropping speed of the second mixed liquid, it is possible to avoid uneven reaction due to excessively high local concentration caused by too fast dropping speed, and unstable reaction due to excessive heat release; it is also possible to avoid extending the entire preparation time due to too slow dropping speed; determine a suitable stirring time for the second mixed liquid to avoid increased energy consumption and reduced production efficiency due to too long stirring time, and to avoid uneven mixing due to too short stirring time, which leads to problems such as uneven particle size distribution and uneven structure after gelation of the silica sol.
[0014] Furthermore, the specific process of removing the gel on the surface of the boron nitride ceramic substrate in step S2 is: using an alkaline solution to adjust the pH value of the silica sol to a weak acid to solidify the silica sol in situ gel, and then heating and drying to treat the gel on the surface of the boron nitride ceramic substrate.
[0015] By adopting the above technical scheme, the hydrolysis reaction rate of tetraethyl orthosilicate is higher than the polycondensation reaction rate under acid catalysis, producing many oligomers and polymers, and then a one-step hydrolysis reaction is carried out under alkaline catalysis. Since the hydrolysis and polycondensation rate of the polymer is faster than that of the oligomer under alkaline conditions, the chain of the polymer continues to grow in all directions, and finally the colloidal cluster particles are cross-linked to form a gel network structure. The gel obtained by this method has a high degree of cross-linking and a large network skeleton strength, which is conducive to maintaining and enhancing the performance of boron nitride.
[0016] Furthermore, the pH value of the silica sol is adjusted to acidic by using a pH adjuster, and the pH adjuster is ammonia water with a concentration of 0.2 mol / L to 0.8 mol / L. After adding ammonia water, the pH value is adjusted to 5 to 7.
[0017] By adopting the above technical scheme, the silica sol is solidified in situ by using ammonia pH regulator to prevent the silicon dioxide nanoparticles originally filled in the pores from accumulating on the outer surface of the boron nitride due to the volatilization of the solvent during the heating and drying process, thereby reducing the filling rate of the pores inside the ceramic. At the same time, ammonia is a weak base, which is conducive to obtaining silicon dioxide nanoparticles with uniform morphology, while other strong base systems are more likely to obtain nanoparticles with larger particle size and irregular morphology. In addition, after high-temperature treatment, ammonia will not have residual alkali metal cations that affect the dielectric properties of boron nitride ceramics.
[0018] Furthermore, after the silica sol in-situ gel is solidified, the temperature is raised from room temperature to 100°C; and the boron nitride ceramic matrix after the surface gel is removed is sintered, the sintering temperature is 500°C to 900°C, the heating rate is 5°C / min to 20°C / min, and the insulation time is 60min to 240min.
[0019] Furthermore, in step S3, the sintered boron nitride ceramic matrix is vacuum impregnated for the second time with an organic silicone resin, wherein the solid content of the organic silicone resin is 20% to 50% and the viscosity is 3 mPa•s to 25 mPa•s.
[0020] By adopting the above technical scheme, silicone resin is used for the second vacuum impregnation. After the first impregnation with silica sol, the surface of the boron nitride ceramic substrate will be covered with a layer of silicon dioxide formed by the solidification of silica sol. The strong interaction between silicone resin and silicon dioxide can significantly improve the adhesion of the silicone resin layer on the surface of the boron nitride ceramic substrate, forming a dense and continuous protective layer, further reducing the water absorption rate of the boron nitride ceramic.
[0021] Furthermore, the second vacuum impregnation time is 1 hour to 12 hours; the drying temperature of the boron nitride ceramic matrix after the second vacuum impregnation is 100° C. to 200° C., and the drying time is 1 hour to 6 hours.
[0022] By adopting the above technical scheme, by selecting a suitable immersion time, it is possible to ensure that the silicone resin can fully penetrate into the micropores and cracks of the boron nitride ceramic matrix to form a uniform coating and fill the pores; by selecting suitable drying parameters, the resin can be effectively cured without destroying the thermal stability of the boron nitride ceramic matrix.
[0023] A boron nitride ceramic with low water absorption rate prepared by the method for preparing the boron nitride ceramic with low water absorption rate as described above, wherein the boron nitride ceramic with low water absorption rate is boiled in boiling water for 3 hours, and its water absorption rate is less than 0.2%.
[0024] Other features and corresponding beneficial effects of the present invention are described in the latter part of the specification, and it should be understood that at least part of the beneficial effects become obvious from the description in the specification of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a process flow chart for the preparation of low water absorption boron nitride ceramics. DETAILED DESCRIPTION like Figure 1 As shown, the present invention is further described below in conjunction with specific embodiments and drawings.
[0026] A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: Boil and then dry the boron nitride ceramic substrate, and perform the first vacuum impregnation in silica sol; the boron nitride ceramic substrate in this embodiment can be a boron nitride ceramic product that can be directly purchased on the market; or it can be a boron nitride ceramic product prepared by using raw materials such as boron oxide using existing preparation methods; S2: removing the gel on the surface of the boron nitride ceramic substrate after the first vacuum impregnation; specifically, after the boron nitride ceramic substrate immersed in the silica sol is in-situ gelled, the temperature is gradually increased to dry and the gel on the surface is removed; S3: sequentially sintering and performing a second vacuum impregnation on the boron nitride ceramic substrate after removing the surface gel; S4: Drying the boron nitride ceramic substrate after the second vacuum impregnation to obtain a boron nitride ceramic with low water absorption.
[0027] By adopting the above technical scheme, the formed boron nitride ceramic matrix is directly boiled, so that the boron oxide in the boron nitride ceramic matrix that is easy to absorb moisture is dissolved in boiling water and then dried, thereby reducing the water absorption rate of the boron nitride ceramic matrix to a certain extent, and then it is placed in silica sol for immersion, so that the nano silicon dioxide particles in the silica sol are filled into the pores of the boron nitride, thereby reducing the porosity of the boron nitride ceramic matrix; then the silicon hydroxyl groups on the surface of the silicon dioxide that are easy to absorb moisture are removed by sintering, and the porosity of the boron nitride ceramic is further reduced by a second vacuum impregnation, so that the boron nitride has better moisture resistance; the whole process is simple, the process is controllable, and it is easy to implement, which is conducive to industrial production, and the prepared boron nitride ceramic has high density, low water absorption, excellent dielectric properties and thermal shock resistance, and can be used to prepare aerospace wave-transparent material components.
[0028] It is worth mentioning that one of the highlights of this application is to directly process the finished boron nitride ceramic matrix on the market or the prepared boron nitride ceramic matrix to improve its water absorption rate. The existing mainstream methods for improving the water absorption rate of boron nitride ceramics are: improving the boron nitride ceramic raw material process; optimizing the sintering process; adding sintering aids, etc. However, improving the boron nitride ceramic raw material process is one of the cost increases, because high-quality boron nitride raw materials are usually expensive, some high-quality boron nitride raw materials may be scarce, and it is difficult to obtain; and the impurity content in the raw materials has an important influence on the performance of boron nitride ceramics, and the need to control the purity of the raw materials means that the complexity and cost of raw material processing will increase; second, the improvement of the water absorption rate of boron nitride ceramics through the synergistic effect between the raw materials is limited, and the effect is not obvious. And optimizing the sintering process, whether it is optimizing the sintering temperature or adopting a more advanced sintering method, will increase the cost; and the requirements for sintering equipment are high, and the complexity of the sintering process may also lead to a decrease in process stability, such as temperature fluctuations, inaccurate atmosphere control, etc., which may affect the performance and quality stability of the final product, and are not suitable for promotion and use. The addition of sintering aids often leads to an increase in costs, because the price of sintering aids is usually high, which will bring significant economic pressure for large-scale production; and the sintering aids may remain in the boron nitride ceramics during the sintering process to form impurity phases, which will then affect the specific properties of the boron nitride ceramics themselves.
[0029] In summary, the existing low water absorption rate operation of boron nitride will bring about the problem of increased cost and insignificant effect. Therefore, the present application directly improves the process on the already formed boron nitride ceramic matrix, greatly reduces the water absorption rate of boron nitride ceramics, and does not introduce complex equipment or operations, which significantly reduces the cost. Because the already formed boron nitride ceramic matrix will first be boiled, the boron oxide that is easy to absorb moisture in the boron nitride ceramic matrix will be dissolved in boiling water. This is the first step to improve the water absorption rate of the boron nitride ceramic matrix; then it is placed in silica sol for the first vacuum impregnation, and the silica sol is initially introduced into the surface and internal micropores of the boron nitride ceramic matrix to reduce the porosity of the surface of the boron nitride ceramic. This is the second step to reduce its water absorption rate; finally, through sintering and the second vacuum impregnation, the filling effect of silica sol on the boron nitride ceramic matrix is strengthened, which is the third step to reduce its water absorption rate. The combination of the three steps ultimately makes the low water absorption rate boron nitride ceramic prepared by the present application have extremely low water absorption rate. In addition, the present application can also directly purchase finished boron nitride ceramic bodies with low water absorption rates, and further reduce the water absorption rate of the finished boron ceramic bodies on the premise of low water absorption rate, so that it can meet the use scenarios in specific fields such as the manufacture of high-frequency microwave devices, greatly saving R&D time and efficiency, and with good results.
[0030] In one embodiment, the preparation of the silica sol in step S1 includes dissolving tetraethyl orthosilicate in ethanol, mixing and stirring to obtain a first mixed liquid, adding a second mixed liquid to the first mixed liquid, mixing and stirring, and then standing to obtain the silica sol; the second mixed liquid is a mixture of hydrochloric acid and water.
[0031] Compared with the traditional method for preparing silica sol, the obtained silica sol has a lower particle size, reaching a single-digit nanometer particle size, while the silica sol prepared by the traditional preparation method is mostly in the tens of nanometers. Smaller particle size is conducive to fully filling the pores of boron nitride ceramics and effectively reducing the porosity. The silica sol obtained by using tetraethyl orthosilicate as a silicon source has the best performance and a relatively stable process. Ethanol is added as a solvent for the hydrolysis of tetraethyl orthosilicate, which will not hinder the hydrolysis and condensation reaction of tetraethyl orthosilicate, and is safer than other alcohols. Water is added as a reactant for the hydrolysis of tetraethyl orthosilicate, and hydrochloric acid is added as a hydrolysis catalyst, which can promote the full completion of the hydrolysis reaction and increase the solid content of the silica sol. The mixed solution is configured in the above order to make the preparation of silica sol reaction more complete. At the same time, the applicant also conducted experiments, and the silica sol prepared above can be stored at room temperature for more than 3 months or even longer before adding ammonia water to adjust the pH value. It has good stability and is easy to store, which is conducive to industrial production.
[0032] Preferably, the molar ratio of tetraethyl orthosilicate: ethanol: water: hydrochloric acid is set to 1: 4 to 20: 4 to 8: 1.0×10-3 to 2.0×10-3; and the pH value of the second mixed solution is 2 to 3. It is explained here that the molar ratio of tetraethyl orthosilicate to water determines the rate and degree of the hydrolysis reaction; ethanol is used as a solvent, and its molar ratio with tetraethyl orthosilicate will affect the particle size of the silica sol; hydrochloric acid is used as a catalyst, and its molar ratio with tetraethyl orthosilicate has an important influence on the rate of the hydrolysis reaction and the stability of the product. Since these four raw materials affect each other, the inventors of this application have reasonably set the molar ratio of the raw materials so that the particle size, distribution, stability, yield and reaction rate of the silica sol can be well taken into account.
[0033] Preferably, in the process of preparing silica sol, the second mixed liquid is added to the first mixed liquid at a dripping speed of 1ml / min to 5ml / min. If the second mixed liquid is dropped too fast, the pH value of the local area in the reaction system will drop rapidly, the polymerization reaction speed of silicate ions will be accelerated, and a large number of fine gel particles may be produced. These particles may aggregate rapidly, resulting in an uneven gel structure and even precipitation; if the drop speed is too slow, the entire reaction time will be prolonged and the generation rate of silica sol will be reduced. The mixing and stirring time after the second mixed liquid is added is 1h to 5h. Insufficient stirring time will lead to uneven mixing between ethanol, tetraethyl orthosilicate, hydrochloric acid and water, affecting the generation and properties of silica sol; too long stirring time will increase energy consumption and reduce production efficiency.
[0034] In one embodiment, the specific process of removing the gel on the surface of the boron nitride ceramic substrate in step S2 is: adjusting the pH value of the silica sol to acidic to solidify the silica sol in situ, and then heating and drying to treat the gel on the surface of the boron nitride ceramic substrate.
[0035] In the present embodiment, the silica sol is in situ gel-cured under acidic conditions, and the polymerization rate of silicates in the silica sol is accelerated, which is conducive to the rapid formation of gel and improves the filling efficiency of the pores of the boron nitride ceramic matrix; and during the in situ gel curing process, the combination of the gel layer and the surface of the boron nitride ceramic matrix may be uniform and controllable, so as to avoid damage to the surface of the boron nitride ceramic matrix during the subsequent cleaning process; at the same time, the curing process does not require high temperature, so the thermal effect on the boron nitride ceramic matrix is small, which helps to maintain its original physical and chemical properties.
[0036] Specifically, in this embodiment, the pH value of the silica sol is adjusted to acidic by using a pH adjusting agent, and the pH adjusting agent is ammonia water, and the concentration of ammonia water is 0.2 mol / L to 0.8 mol / L. After adding ammonia water, the pH value is adjusted to 5 to 7. By using ammonia water pH adjusting agent to solidify the silica sol in situ gel, it is prevented that the silicon dioxide nanoparticles originally filled in the pores are driven to accumulate on the outer surface of the boron nitride during the temperature increase and drying process due to the volatilization of the solvent, thereby reducing the filling rate of the pores inside the ceramic; at the same time, ammonia water has low toxicity and volatility, and relatively little pollution to the environment, and more importantly, ammonia water will not have residual alkali metal cations after high-temperature treatment to affect the dielectric loss of the boron nitride ceramic.
[0037] In one embodiment, the temperature of the silica sol in-situ gel is raised from room temperature to 100°C after solidification; and the boron nitride ceramic matrix after removing the surface gel is sintered, the sintering temperature is 500°C to 900°C, the heating rate is 5°C / min to 20°C / min, and the insulation time is 60min to 240min; determine appropriate sintering parameters so that the bonding force between the boron nitride particles is enhanced, the particle surface melts, and a denser bond is formed, which helps to improve the density and mechanical properties of the ceramic; at the same time, it does not generate excessive production costs and energy consumption. The drying temperature of the boron nitride ceramic matrix after the second vacuum impregnation is 100°C to 200°C, and the drying time is 1h to 6h. The appropriate drying temperature and drying time can ensure that the boron nitride ceramic will not cause thermal stress, cracking or performance degradation due to excessive temperature while removing solvents or moisture.
[0038] In one embodiment, in step S3, the sintered boron nitride ceramic substrate is vacuum impregnated for the second time with an organic silicone resin, the solid content of the organic silicone resin is 20% to 50%, and the viscosity is 3 mPa•s to 25 mPa•s; the time for the second vacuum impregnation is 1 hour to 12 hours.
[0039] Specifically, it is explained here that before the second vacuum impregnation, the boron nitride ceramic matrix has been subjected to the first vacuum impregnation, and the pores inside the boron nitride ceramic matrix have been basically filled with silica sol; therefore, the purpose of the second vacuum impregnation is to strengthen the filling effect of silica sol on the boron nitride ceramic matrix, which can ensure that more silica sol penetrates into the micropores and cracks of the boron nitride ceramic matrix, and further reduce its water absorption rate; and the second vacuum impregnation uses silicone resin because the strong interaction between silicone resin and silica in silica sol can significantly improve the adhesion of the silicone resin layer on the surface of the boron nitride ceramic, and this strong adhesion ensures that the resin layer can be firmly attached to the ceramic surface and is not easy to fall off or crack; at the same time, the close combination between silicone resin and silica forms a dense and continuous protective layer, which can effectively block the penetration of moisture and other corrosive media, and further reduce the water absorption rate of the boron nitride ceramic.
[0040] If silica sol is used for the second impregnation, although silica sol can fill the micropores and defects on the surface of the boron nitride ceramic matrix, a single silica sol layer may not be able to completely prevent the penetration of water, and the purpose of low water absorption cannot be achieved; if organic resin is used for both vacuum impregnations, although the protective film formed by the silicone resin has high density and water resistance, an overly thick resin layer will affect the air permeability and other properties of the boron nitride ceramic, making it impossible to use it in some high-frequency microwave devices, and its applicability will be poor.
[0041] A low water absorption boron nitride ceramic prepared by the preparation method of low water absorption boron nitride ceramic as described above, wherein the water absorption of the low water absorption boron nitride ceramic is less than 0.2%, and while ensuring extremely low water absorption, the ceramic has good thermal shock resistance, a small dielectric constant, low dielectric loss, and good high temperature oxidation resistance, and can be applied to the field of high temperature resistant and wave-transmitting ceramics.
[0042] Example 1 A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: After the homemade boron nitride ceramic substrate with a density of 90% was boiled in boiling water for 5 hours and completely dried, it was completely immersed in silica sol for the first vacuum impregnation for 3 hours, and the vacuum degree was -0.09MPa; the silica sol was prepared as follows: 208g of tetraethyl orthosilicate was weighed and dissolved in 276g of ethanol solvent, and then a mixed solution of 72g of water and 133μL of concentrated hydrochloric acid was slowly added at a dropping speed of 1ml / min, wherein the molar ratio of tetraethyl orthosilicate: ethanol: water: concentrated hydrochloric acid was 1:6:4:1.6×10-3, and the silica sol solution was obtained after stirring for 2 hours and then standing; S2: After the boron nitride ceramic substrate immersed in the silica sol is in-situ gelled, the temperature is gradually increased to dry and the surface gel is removed; that is, the pH value of the silica sol is adjusted to 6.5 with an ammonia solution with a concentration of 0.5 mol / L, and the silica sol is allowed to stand for 20 minutes to solidify the in-situ gel of the silica sol, and then the temperature is gradually increased from room temperature to 100°C in an oven to dry, and then the surface gel of the boron nitride ceramic substrate is removed; S3: After removing the surface gel, the boron nitride ceramic substrate is dried in an oven from room temperature to 100°C, then placed in a muffle furnace and heated to 700°C at a heating rate of 8°C / min for sintering for 150 minutes. After cooling, the substrate is placed in a silicone resin with a solid content of 30% and a viscosity of 10 mPa•s and vacuum immersed for 3 hours. S4: After the second vacuum impregnation, the boron nitride ceramic substrate is taken out and placed in a 120° C. oven for drying for 3 hours to obtain a low water absorption boron nitride ceramic.
[0043] The obtained low water absorption boron nitride ceramics were boiled in boiling water for 3 hours. The water absorption of the obtained low water absorption boron nitride ceramics was tested to be only 0.03%, while the water absorption of the finished commercially available boron nitride ceramics without any treatment was 4.89%, indicating that the water absorption of the boron nitride ceramics treated by this method was significantly reduced. At the same time, the obtained boron nitride ceramics were directly placed in a muffle furnace at 1000°C for 20 minutes of high temperature insulation, and then directly taken out and thrown into cold water. No cracking occurred, indicating that the boron nitride ceramics had good thermal shock resistance. In addition, the dielectric properties of the low water absorption boron nitride ceramics were tested, with a dielectric constant of 4.6 and a dielectric loss of 1.0×10-3, indicating that the boron nitride ceramics treated by this method still had good dielectric properties.
[0044] Example 2 A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: After the homemade boron nitride ceramic substrate with a density of 90% was boiled in boiling water for 5 hours and completely dried, it was completely immersed in silica sol for the first vacuum impregnation for 3 hours, and the vacuum degree was -0.09MPa; the silica sol was prepared as follows: 208g of tetraethyl orthosilicate was weighed and dissolved in 276g of ethanol solvent, and then a mixed solution of 72g of water and 133μL of concentrated hydrochloric acid was slowly added at a dropping speed of 1ml / min, wherein the molar ratio of tetraethyl orthosilicate: ethanol: water: concentrated hydrochloric acid was 1:6:4:1.6×10-3, and the silica sol solution was obtained after stirring for 2 hours and then standing; S2: removing the gel on the surface of the boron nitride ceramic substrate after the first vacuum impregnation; that is, gradually raising the temperature from room temperature to 100° C. in an oven to solidify and dry the gel, and then removing the gel on the surface of the boron nitride ceramic substrate; S3: After removing the surface gel, the boron nitride ceramic substrate is dried in an oven from room temperature to 100°C, then placed in a muffle furnace and heated to 700°C at a heating rate of 8°C / min for sintering for 150 minutes. After cooling, the substrate is placed in a silicone resin with a solid content of 30% and a viscosity of 10 mPa•s and vacuum immersed for 3 hours. S4: After the second vacuum impregnation, the boron nitride ceramic substrate is taken out and placed in a 120° C. oven for drying for 3 hours to obtain a low water absorption boron nitride ceramic.
[0045] The obtained low water absorption boron nitride ceramics were boiled in boiling water for 3 hours. The water absorption of the obtained low water absorption boron nitride ceramics was tested to be 1.26%. This shows that compared with the silica sol gel curing by solvent evaporation, the silica sol in-situ gel curing has higher pore filling efficiency and lower water absorption.
[0046] Example 3 A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: After the homemade boron nitride ceramic substrate with a density of 95% was boiled in boiling water for 5 hours and completely dried, it was completely immersed in silica sol for the first vacuum impregnation for 2 hours, and the vacuum degree was -0.09MPa; the silica sol was prepared as follows: 208g of tetraethyl orthosilicate was weighed and dissolved in 368g of ethanol solvent, and then a mixed solution of 108g of water and 150μL of concentrated hydrochloric acid was slowly added at a dropping speed of 2ml / min, wherein the molar ratio of tetraethyl orthosilicate: ethanol: water: concentrated hydrochloric acid was 1:8:6:1.8×10-3, and the silica sol solution was obtained after stirring for 1h and standing; S2: removing the surface gel of the boron nitride ceramic substrate after the first vacuum impregnation; that is, adjusting the pH value of the silica sol to 7.0 with an ammonia solution with a concentration of 0.5 mol / L, and after standing for 10 minutes, the silica sol is in-situ gelled and solidified, and the surface gel of the boron nitride ceramic substrate is removed; S3: After removing the surface gel, the boron nitride ceramic substrate is dried in an oven from room temperature to 100°C, then placed in a muffle furnace and heated to 750°C at a heating rate of 10°C / min for sintering for 120 min. After cooling, the substrate is placed in a silicone resin with a solid content of 35% and a viscosity of 10 mPa•s and vacuum immersed for 3 h. S4: After the second vacuum impregnation, the boron nitride ceramic substrate is taken out and placed in a 150° C. oven for drying for 2 hours to obtain a boron nitride ceramic with low water absorption.
[0047] The obtained low water absorption boron nitride ceramics were boiled in boiling water for 3 hours, and the water absorption of the obtained low water absorption boron nitride ceramics was tested to be only 0.13%. Example 4 A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: After the homemade boron nitride ceramic substrate with a density of 92% was boiled in boiling water for 5 hours and completely dried, it was completely immersed in silica sol for the first vacuum impregnation for 3 hours, and the vacuum degree was -0.09MPa; the silica sol was prepared as follows: 208g of tetraethyl orthosilicate was weighed and dissolved in 184g of ethanol solvent, and then a mixed solution of 72g of water and 133μL of concentrated hydrochloric acid was slowly added at a dropping speed of 2ml / min, wherein the molar ratio of tetraethyl orthosilicate: ethanol: water: concentrated hydrochloric acid was 1:4:4:1.6×10-3, and the silica sol solution was obtained after stirring for 2 hours and then standing; S2: removing the surface gel of the boron nitride ceramic substrate after the first vacuum impregnation; that is, adjusting the pH value of the silica sol to 6.0 with an ammonia solution with a concentration of 0.3 mol / L, and after standing for 3 hours, the silica sol is in-situ gelled and solidified, and the surface gel of the boron nitride ceramic substrate is removed; S3: After removing the surface gel, the boron nitride ceramic substrate is placed in a muffle furnace and heated to 850°C at a rate of 10°C / min for sintering for 120 min. After cooling, it is placed in a silicone resin with a solid content of 40% and a viscosity of 15 mPa•s and vacuum immersed for 3 h. S4: After the second vacuum impregnation, the boron nitride ceramic substrate is taken out and placed in a 150° C. oven for drying for 2 hours to obtain a boron nitride ceramic with low water absorption.
[0048] The obtained low water absorption boron nitride ceramics were boiled in boiling water for 3 hours, and the water absorption of the obtained low water absorption boron nitride ceramics was tested to be only 0.15%.
[0049] Example 5 A method for preparing boron nitride ceramics with low water absorption rate comprises the following steps: S1: After the homemade boron nitride ceramic substrate with a density of 90% was boiled in boiling water for 5 hours and completely dried, it was completely immersed in silica sol for the first vacuum impregnation for 3 hours, and the vacuum degree was -0.09MPa; the silica sol was prepared as follows: 208g of tetraethyl orthosilicate was weighed and dissolved in 552g of ethanol solvent, and then a mixed solution of 144g of water and 266μL of concentrated hydrochloric acid was slowly added at a dropping speed of 2ml / min, wherein the molar ratio of tetraethyl orthosilicate: ethanol: water: concentrated hydrochloric acid was 1:12:8:1.6×10-3, and the silica sol solution was obtained after stirring for 2 hours and then standing; S2: removing the surface gel of the boron nitride ceramic substrate after the first vacuum impregnation; that is, adjusting the pH value of the silica sol to 5.8 with an ammonia solution with a concentration of 0.3 mol / L, and after standing for 4 hours, the silica sol is in-situ gelled and solidified, and the surface gel of the boron nitride ceramic substrate is removed; S3: After removing the surface gel, the boron nitride ceramic substrate is placed in a muffle furnace and heated to 850°C at a heating rate of 10°C / min for sintering for 180 min. After cooling, it is placed in a silicone resin with a solid content of 45% and a viscosity of 20 mPa•s and vacuum immersed for 3 h. S4: After the second vacuum impregnation, the boron nitride ceramic substrate is taken out and placed in a 150° C. oven for drying for 2 hours to obtain a boron nitride ceramic with low water absorption.
[0050] The obtained low water absorption boron nitride ceramics were boiled in boiling water for 3 hours, and the water absorption of the obtained low water absorption boron nitride ceramics was tested to be only 0.19%.
[0051] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that during the first vacuum impregnation, the finished boron nitride ceramic matrix is not boiled, and the first vacuum impregnation is directly carried out in silica sol, and the other operating conditions and steps are the same as those of Example 1. The boron nitride ceramic finally obtained in Comparative Example 1 is boiled in boiling water for 3 hours, and the water absorption rate of the obtained boron nitride ceramic is 1.03%, which indicates that the boron nitride ceramic matrix that has not been boiled still contains boron oxide that is easy to absorb moisture, and the water absorption rate of the boron nitride ceramic will increase after boiling in boiling water.
[0052] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that during the first vacuum impregnation, the boron nitride ceramic matrix is vacuum impregnated with an organic silicon resin, and the other operating conditions and steps are the same as those of Example 1. The boron nitride ceramic finally obtained in Comparative Example 2 was boiled in boiling water for 3 hours, and the water absorption rate of the obtained boron nitride ceramic was 2.28%, which shows that the boron nitride ceramic matrix itself has a self-lubricating effect, and the interaction between the organic silicon resin and the boron nitride ceramic matrix is weak, so the pores in the boron nitride ceramic matrix cannot be filled. Silica sol is used for the first vacuum impregnation, and the surface obtained after the nano-silica in the silica sol is filled with pores and sintered at high temperature is silica, which has a stronger interaction with the organic silicon resin, so the pore filling rate is better.
[0053] The examples described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should all fall within the protection scope of the present invention.
Claims
1. A method for preparing boron nitride ceramics with low water absorption, Features: The steps include: S1: Boil and dry the boron nitride ceramic substrate, and perform the first vacuum impregnation in silica sol; S2: removing the gel on the surface of the boron nitride ceramic substrate immersed in the silica sol; S3: sequentially sintering and vacuum impregnating the boron nitride ceramic substrate after removing the surface gel; wherein the second vacuum impregnation is performed on the boron nitride ceramic substrate after removing the surface gel using an organic silicone resin; S4: Drying the boron nitride ceramic substrate after the second vacuum impregnation to obtain a boron nitride ceramic with low water absorption.
2. A method for preparing a low water absorption boron nitride ceramic according to claim 1, Features: The preparation of the silica sol in step S1 includes dissolving tetraethyl orthosilicate in ethanol, mixing and stirring to obtain a first mixed liquid, adding a second mixed liquid to the first mixed liquid, mixing and stirring, and then standing to obtain the silica sol; the second mixed liquid is a mixture of hydrochloric acid and water.
3. A method for preparing a low water absorption boron nitride ceramic according to claim 2, Features: The molar ratio of tetraethyl orthosilicate: ethanol: water: hydrochloric acid is 1:4-20:4-8:1.0×10 -3 ~2.0×10 -3 ; and the pH value is 2-3 after adding the second mixed solution.
4. A method for preparing a low water absorption boron nitride ceramic according to claim 2 or 3, Features: The second mixed liquid is added to the first mixed liquid at a dropping speed of 1 ml / min to 5 ml / min, and the mixing and stirring time after the second mixed liquid is added is 1 h to 5 h.
5. The method for preparing a low water absorption boron nitride ceramic according to claim 1, Features: The specific process of removing the gel on the surface of the boron nitride ceramic substrate in step S2 is: adjusting the pH value of the silica sol to weak acidity to solidify the silica sol in situ gel, and then heating and drying to treat the gel on the surface of the boron nitride ceramic substrate.
6. A method for preparing a low water absorption boron nitride ceramic according to claim 5, Features: The pH value of the silica sol is adjusted to weak acidity by using an alkaline solution pH regulator, and the pH regulator is ammonia water with a concentration of 0.2 mol / L to 0.8 mol / L. After adding ammonia water, the pH value is adjusted to 5 to 7.
7. A method for preparing a low water absorption boron nitride ceramic according to claim 6, Features: After the silica sol in-situ gel is solidified, the temperature is raised from room temperature to 100°C; and the boron nitride ceramic matrix after the surface gel is removed is sintered, the sintering temperature is 500°C to 900°C, the heating rate is 5°C / min to 20°C / min, and the insulation time is 60min to 240min.
8. The method for preparing a low water absorption boron nitride ceramic according to claim 1, Features: In the step S3, the sintered boron nitride ceramic matrix is vacuum impregnated for the second time with an organic silicone resin, wherein the solid content of the organic silicone resin is 20% to 50% and the viscosity is 3 mPa·s to 25 mPa·s.
9. A method for preparing a low water absorption boron nitride ceramic according to claim 8, Features: The time of the second vacuum impregnation is 1 hour to 12 hours; the drying temperature of the boron nitride ceramic matrix after the second vacuum impregnation is 100° C. to 200° C., and the drying time is 1 hour to 6 hours.
10. A boron nitride ceramic with low water absorption prepared by the method for preparing a boron nitride ceramic with low water absorption as claimed in any one of claims 1 to 9, Features: The water absorption rate of the low water absorption rate boron nitride ceramic is less than 0.2%.
Citation Information
Patent Citations
Boron nitride and silicon dioxide composite ceramic aerogel and preparation method thereof
CN116425554A
Hole sealing moisture-proof anticorrosive composite coating material and its prepn process
CN1931795A
Resin-impregnated boron nitride body and a method for producing the same
EP3326990A1
Cited By
Porous boron nitride antenna window and hole sealing coating method thereof
CN119143523A
High-temperature-resistant electric connector and preparation method thereof
CN119481792A
Preparation method of special-shaped thin-wall porous material airtight coating
CN121405503A
A method for preparing a profiled thin-walled porous material gas-tight coating
CN121405503B