Preparation method of vinyl silane coupling agent
By using platinum catalyst and hydrogen chloride reuse technology, the problems of long reaction time and waste of resources in the preparation of vinyl silane coupling agents are solved, and the preparation of vinyl silane coupling agents with high selectivity and high yield is achieved, which improves the product stability and resource utilization.
Patent Information
- Application Number
- CN202410801495.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-05
AI Technical Summary
The existing preparation methods for vinyl silane coupling agents have problems such as long reaction time, low product yield and waste of resources. In particular, copper-based catalysts are prone to agglomeration under high temperature conditions, which affects the reaction rate and yield.
Using a composite network composed of crosslinked carbon nanofibers and end amino hyperbranched polymers, the reaction time is shortened, the selectivity and yield are improved, and the distillation residue is carried out through catalyst pre-activation and hydrogen chloride reuse technology. Recycling reduces by-products and improves resource utilization.
The high selectivity and high yield of vinyl silane coupling agent is achieved, the reaction time is reduced, the side reaction is reduced, the recycling rate of resources is improved, and the stability and catalytic efficiency of the product are improved.
Abstract
Description
Technical Field
[0001] The invention relates to the field of silane coupling agents, and in particular to a method for preparing a vinyl silane coupling agent. Background Art
[0002] Vinyl silane coupling agents can chemically combine with both inorganic and organic materials, and are mainly used in glass fiber surface treatment, resin modification, polyethylene cross-linking, etc. At present. The acetylene method is widely used to prepare vinyl silane coupling agents. This method is: acetylene and trichlorosilane are used in the presence of a catalyst to synthesize vinyl trichlorosilane through a hydrosilylation reaction. This method does not release hydrogen chloride, and has the advantages of mild reaction conditions and good reaction activity, but the hydrosilylation method is also prone to secondary reactions, which affects the selectivity and yield of the final vinyl silane coupling agent. Therefore, how to improve the selectivity and yield of vinyl silane coupling agents is a technical difficulty that needs to be overcome.
[0003] Patent CN117384203A discloses a method for preparing a vinyl trimethoxysilane coupling agent and its application. The method uses silicon powder and methanol to mix, react under the action of a first catalyst to obtain trimethoxysilane, and then mix the trimethoxysilane with acetylene and an organic solvent to react, obtain a mixture under the action of a second catalyst, and separate and obtain vinyl trimethoxysilane through hydrogen treatment and distillation. However, the method also has the following shortcomings: the first catalyst used is a copper catalyst, and the silicon powder and methanol need to be heated to react. The copper catalyst is easy to agglomerate under high temperature conditions, which affects the reaction rate and the yield of trichlorosilane, thereby affecting the yield of the vinyl trimethoxysilane coupling agent; the method uses a lot of solvents, which will produce more by-products accordingly, and the method does not involve the recovery and treatment of by-products, resulting in a waste of resources.
[0004] Therefore, finding a method for preparing a vinyl silane coupling agent that has a fast reaction speed, is green and environmentally friendly, saves resources and has a high yield is a problem that needs to be solved at present. Summary of the invention
[0005] In order to solve the above-mentioned technical problems of long reaction time, low product yield and waste of resources, the present invention provides a method for preparing a vinyl silane coupling agent. By designing the catalyst, the reaction time can be shortened, the proportion of side reactions can be reduced, the reaction selectivity can be improved, and the conversion rate can be higher, thereby improving the product yield; a by-product recovery and processing process is designed to achieve the recycling of resources.
[0006] The specific technical scheme of the present invention is: A method for preparing a vinyl silane coupling agent comprises the following steps: S1: reacting silicon powder with hydrogen chloride, and subjecting the product to purification treatment including distillation to obtain trichlorosilane and a distillation residue containing silicon tetrachloride; S2: pre-activating the catalyst, reacting trichlorosilane with acetylene under the action of the activated catalyst and an inert solvent, separating and purifying the product to obtain vinyl trichlorosilane; S3: reacting vinyltrichlorosilane with alcohol, separating and purifying the product to obtain a vinylsilane coupling agent, recovering the hydrogen chloride gas generated during the reaction, and recycling the hydrogen chloride gas to step S1 after purification treatment including washing with distillation residue containing silicon tetrachloride.
[0007] First, trichlorosilane is prepared by silicon powder and hydrogen chloride, then organochlorosilane is prepared by hydrogen-silicon addition reaction, and then the organochlorosilane is alcoholyzed and esterified to finally prepare a vinyl silane coupling agent. The main reaction chemical formula of the present invention is as follows: S1:Si+3HCl=SiHCl3+H2 S2: HC≡CH+HSiCl3→CH2=CHSiCl3 S3: C2H3SiCl3+3CH3OH→C2H3Si(OCH3)3+3HCl C2H3SiCl3+3C2H5OH→C2H3Si(OC2H5)3+3HCl (taking methanol and ethanol as examples, the choice of alcohol can be adjusted according to the type of vinyl silane coupling agent to be prepared) For the hydrogen silicon addition reaction, the catalyst pre-activation process is added to improve the activity and stability of the catalyst, shorten the reaction time, and improve the reaction selectivity. A large amount of hydrogen chloride gas will be produced during the alcoholysis and esterification of organochlorosilane. Hydrogen chloride has a large solubility in vinyl silane, which is not conducive to the hydrolysis and condensation of vinyl silane coupling agent, and affects the use of vinyl silane coupling agent. The present invention designs a hydrogen chloride recycling process. The distillation residue obtained in step S1 contains silicon tetrachloride, a by-product in the hydrogen silicon synthesis process. The distillation residue is used to wash the hydrogen chloride, which can remove the moisture in the hydrogen chloride. At the same time, the silicon tetrachloride impurities are recycled to step S1 with the hydrogen chloride, which can inhibit the occurrence of side reactions, thereby achieving the purpose of improving the production efficiency of trichlorosilane, and can also realize the recycling of resources, that is, the distillation residue after distillation is recycled, which can improve the yield of trichlorosilane product.
[0008] Preferably, the catalyst used in S2 is a platinum catalyst; the platinum catalyst includes a composite network consisting of mutually cross-linked carbon nanofibers and amino-terminated hyperbranched polymers, and a platinum element bound to the amino-terminated hyperbranched polymer; the amino-terminated hyperbranched polymer is covalently bonded to the surface of the carbon nanofibers through amide bonds, so that connections are formed between the carbon nanofibers.
[0009] The catalyst used in the hydrosilylation reaction process contains a composite network composed of carbon nanofibers and amino-terminated hyperbranched polymers. The carbon nanofibers are connected by the amino-terminated hyperbranched polymers. This structure confines the carbon nanofibers in a certain space, which is conducive to the contact between the carbon nanofibers to form a heat-conducting network, and quickly conducts the heat released during the reaction to the outside, thereby reducing the problem of aggravation of side reactions due to local overheating, improving the reaction selectivity, and then improving the yield. At the same time, the amino-terminated hyperbranched polymer contains more amino groups, which are binding sites for platinum elements. Therefore, there are more catalytic active sites in the platinum catalyst, which can play a better catalytic role.
[0010] In addition, in the platinum catalyst, carboxyl groups can be formed on the surface of the carbon nanofibers by a conventional surface oxidation method, and the carboxyl groups are used to react with the amino groups in the amino-terminated hyperbranched polymer to form amide bonds, thereby realizing covalent bonds between the carbon nanofibers and the amino-terminated hyperbranched polymers, and the amino-terminated hyperbranched polymers are combined with platinum elements as catalytic active sites, so that the platinum catalyst has good stability and can still maintain high selectivity and catalytic efficiency when repeatedly used. The amino-terminated hyperbranched polymer is a copolymer of triethylenetetramine and methyl acrylate.
[0011] Preferably, in the platinum catalyst, the mass ratio of carbon nanofibers to amino-terminated hyperbranched polymers is 1:(0.2-0.4).
[0012] In the above platinum catalyst, within a certain range, the proportion of the amino-terminated hyperbranched polymer increases, which helps the carbon nanofibers to contact each other and form a heat-conducting network; but when its proportion exceeds a certain range and continues to increase, it will block the direct contact between the carbon nanofibers, which is not conducive to the formation of a heat-conducting network. Based on this, controlling the mass ratio of carbon nanofibers to amino-terminated hyperbranched polymers within the range of 1: (0.2-0.4) can improve the selectivity of the platinum catalyst-catalyzed hydrosilylation reaction to a greater extent.
[0013] Preferably, the inert solvent used in S2 is xylene.
[0014] Preferably, the silicon powder and hydrogen chloride in S1 react in a reactor, and the silicon powder is added to the reactor at a flow rate of 60 to 80 kg / h, and the hydrogen chloride is added to the reactor at a flow rate of 140 to 200 nm3 / h.
[0015] Preferably, the reaction temperature of the reactor in S1 is 280-310° C., and the reaction pressure is 0.5-0.7 MPa.
[0016] Preferably, in S1, a pressure swing adsorption device is used to extract the hydrogen generated by the reaction.
[0017] Preferably, the acetylene and trichlorosilane in S2 react in a reactor, and acetylene is added to the reactor at a flow rate of 30 to 40 kg / h, and trichlorosilane is added to the reactor at a flow rate of 75 to 110 kg / h.
[0018] Preferably, the solvent in S2 is added to the reactor at a flow rate of 70 to 100 kg / h.
[0019] Preferably, the reaction temperature of the reactor in S2 is 80-120° C., and the reaction pressure is 80-120 kPa.
[0020] Preferably, in S3, the vinyltrichlorosilane and the alcohol react in a reactor, and the vinyltrichlorosilane is added to the reactor at a flow rate of 90 to 130 kg / h, and the alcohol is added to the reactor at a flow rate of 60 to 100 kg / h.
[0021] Preferably, the reaction temperature of the reactor in S3 is 100 to 120° C., and the reaction pressure is -8 to -4 kPa.
[0022] Preferably, in S1, the reactor used is a synthesis kettle, the silicon powder is dried and reacted with hydrogen chloride in the synthesis kettle, the generated hydrogen is recovered, the remaining products are cooled by cooling water, deep cooled by -40 to -35°C refrigerant, the first distillation tower removes dichlorosilane, the second distillation tower removes silicon tetrachloride, and high-purity trichlorosilane is obtained.
[0023] Preferably, in S2, the reactor used is an ultra-gravity reactor, acetylene is dried and reacted with trichlorosilane in an ultra-gravity reactor to obtain a product under the action of an activated catalyst and an inert solvent, the gas produced by the reaction is condensed into a tail gas recovery tank through two stages, and the product is distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain high-purity vinyltrichlorosilane.
[0024] Preferably, in S3, the reactor used is an esterification reaction tower, the alcohol liquid is vaporized and reacted with vinyl trichlorosilane in the esterification reaction tower, the hydrogen chloride gas generated in the reaction process is placed in a pressure vessel, washed with a supergravity reactor and distillation residue, condensed in two stages, demisted, and distilled to obtain high-purity hydrogen chloride, which is recycled to the synthesis kettle to react with silicon powder; the remaining product is partially refluxed to the esterification reaction tower through a material reflux pump, and partially enters a neutralization kettle to be neutralized with sodium alcohol, and the neutralized product enters a distillation tower for distillation to obtain a high-purity vinyl silane coupling agent, and the by-product separated by distillation is returned to the esterification reaction tower to react with alcohol.
[0025] The preparation method of the platinum catalyst used in the present invention is as follows: 1) covalently cross-linking the amino-terminated hyperbranched polymer and the carbon nanofiber to prepare a composite; 2) Combine platinum element with the complex to produce a platinum catalyst.
[0026] Preferably, step 1) specifically includes the following steps: carbon nanofibers are surface oxidized to obtain carboxylated carbon nanofibers, which are dispersed in a condensation reaction solvent, and a mixed solution of a hyperbranched polymer containing terminal amino groups and a condensation agent is added to carry out a condensation reaction, and the product is separated to obtain a composite.
[0027] In the above process, the condensation agent can activate the carboxyl group, promote the carboxyl group and the amino group to form an amide bond through a condensation reaction, realize the covalent bond between the carbon nanofibers and the amino-terminated hyperbranched polymer, and form a connection between the carbon nanofibers.
[0028] Preferably, in step 1), the preparation method of the amino-terminated hyperbranched polymer comprises the following steps: under the protection of an inert gas, methyl acrylate is added dropwise to a mixture of triethylenetetramine and an addition reaction solvent, the temperature is controlled below 10°C, the mixture is heated to 20-35°C and reacted for 3-4 hours, the addition reaction solvent is removed by rotary evaporation under reduced pressure, and the mixture is heated to 100-110°C and reacted for 2-3 hours to obtain an amino-terminated hyperbranched polymer.
[0029] Preferably, step 2) specifically comprises the following steps: dispersing the complex into a 1-5 wt% chloroplatinic acid solution, separating the product after sufficient adsorption to obtain a platinum catalyst.
[0030] Compared with the prior art, the present invention has the following advantages: (1) Adding a hydrogen chloride recycling process, the hydrogen chloride gas produced in the alcoholysis and esterification process of organic chlorosilane is purified by washing the distillation residue and then put into the trichlorosilane preparation process. On the one hand, it can inhibit the occurrence of side reactions, thereby achieving the purpose of improving the production efficiency of trichlorosilane. On the other hand, it can realize the recycling of by-products. The kettle liquid after distillation can be recycled to increase the yield of trichlorosilane products, thereby increasing the yield of vinyl silane coupling agent.
[0031] (2) The catalyst is optimized. The platinum catalyst used includes a composite network composed of mutually cross-linked carbon nanofibers and amino-terminated hyperbranched polymers, and a platinum element bound to the amino-terminated hyperbranched polymer. The catalyst can accelerate heat dissipation during the hydrosilylation reaction, thereby improving the reaction selectivity and further improving the yield; the platinum catalyst has a large number of catalytic active sites and can exert a good catalytic effect. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the embodiments.
[0033] Overall embodiment A method for preparing a vinyl silane coupling agent comprises the following steps: S1: reacting silicon powder with hydrogen chloride, purifying and distilling the product to obtain trichlorosilane and distillation residue; S2: pre-activating the catalyst, reacting trichlorosilane with acetylene under the action of the activated catalyst and an inert solvent, separating and purifying the product to obtain vinyl trichlorosilane; S3: reacting vinyl trichlorosilane with alcohol, separating and purifying the product to obtain a vinyl silane coupling agent, recovering the hydrogen chloride gas generated during the reaction, and mixing the hydrogen chloride gas with silicon powder for reaction after purification treatment including washing with distillation residue. As a specific embodiment, the catalyst used in S2 is a platinum catalyst, and the platinum catalyst includes a composite network composed of cross-linked carbon nanofibers and amino-terminated hyperbranched polymers, and the amino-terminated hyperbranched polymers are covalently bonded to the surface of the carbon nanofibers through amide bonds, so that the carbon nanofibers are connected to each other, and the platinum element is combined with the amino-terminated hyperbranched polymer.
[0034] As a specific embodiment, the amino-terminated hyperbranched polymer in the platinum catalyst used in S2 is a copolymer of triethylenetetramine and methyl acrylate.
[0035] As a specific implementation manner, the mass ratio of carbon nanofibers to amino-terminated hyperbranched polymers in the platinum catalyst used in S2 is 1:(0.2-0.4).
[0036] As a specific implementation, the diameter of the carbon nanofibers in the platinum catalyst used in S2 is 50-300 nm, and the length is 30-100 μm.
[0037] As a specific implementation, the inert solvent used in S2 is xylene.
[0038] As a specific embodiment, the silicon powder and hydrogen chloride in S1 react in a reactor, the silicon powder at a flow rate of 60 to 80 kg / h, and the hydrogen chloride at a flow rate of 140 to 200 nm. 3 / h was added to the reactor.
[0039] As a specific implementation, the reaction temperature of the reactor in S1 is 280-310° C., and the reaction pressure is 0.5-0.7 MPa.
[0040] As a specific implementation, in S1, a pressure swing adsorption device is used to extract the hydrogen generated by the reaction.
[0041] As a specific implementation, acetylene and trichlorosilane in S2 react in a reactor, acetylene is added to the reactor at a flow rate of 30-40 kg / h, and trichlorosilane is added to the reactor at a flow rate of 75-110 kg / h.
[0042] As a specific implementation, the solvent in S2 is added to the reactor at a flow rate of 70 to 100 kg / h.
[0043] As a specific implementation, the reaction temperature of the reactor in S2 is 80-120° C., and the reaction pressure is 80-120 kPa.
[0044] As a specific implementation, the catalyst pre-activation process in S2 is to first dissolve the catalyst in a solvent and then introduce acetylene gas for activation.
[0045] As a specific implementation, the vinyltrichlorosilane and alcohol in S3 react in a reactor, and the vinyltrichlorosilane is added to the reactor at a flow rate of 90 to 130 kg / h, and the alcohol is added to the reactor at a flow rate of 60 to 100 kg / h.
[0046] As a specific implementation manner, the reaction temperature of the reactor in S3 is 100 to 120° C., and the reaction pressure is -8 to -4 kPa.
[0047] The method for preparing the platinum catalyst used in the above-mentioned method for preparing the vinyl silane coupling agent comprises the following steps: 1) covalently cross-linking the amino-terminated hyperbranched polymer and the carbon nanofiber to prepare a composite; 2) Combine platinum element with the complex to produce a platinum catalyst.
[0048] As a specific implementation, step 1) specifically includes the following steps: after surface oxidation of carbon nanofibers to obtain carboxylated carbon nanofibers, disperse them in a condensation reaction solvent, add a solution containing an amino-terminated hyperbranched polymer and a condensation agent, perform a condensation reaction, separate the product, and obtain a complex. The condensation agent is 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate (HATU); the mass volume ratio of the carboxylated carbon nanofibers, the condensation agent, and the condensation reaction solvent is 100g:30-60g:1000-1500mL; in the solution containing an amino-terminated hyperbranched polymer and a condensation agent, the content of the amino-terminated hyperbranched polymer is 5-10g / mL; the temperature of the condensation reaction is 80-90°C, and the time is 4-6h.
[0049] As a specific implementation, the surface oxidation specifically includes the following steps: dispersing the carbon nanofibers in a 30-35wt% nitric acid solution, oxidizing at 60-70°C for 1-2h, and separating the product.
[0050] As a specific implementation, step 2) specifically includes the following steps: dispersing the complex into a 1-5wt% chloroplatinic acid solution according to a mass volume ratio of 100g:4000-5000mL, separating the product after sufficient adsorption to obtain a platinum catalyst.
[0051] As a specific embodiment, in step 1), the preparation method of the amino-terminated hyperbranched polymer comprises the following steps: adding methyl acrylate dropwise to a mixture of triethylenetetramine and an addition reaction solvent at a temperature below 10°C and under the protection of an inert gas, reacting at 20 to 35°C for 3 to 4 hours, removing the addition reaction solvent by vacuum rotary evaporation, and reacting at 100 to 110°C for 2 to 3 hours to obtain an amino-terminated hyperbranched polymer. The molar ratio of triethylenetetramine to methyl acrylate is 1:0.8 to 1.2. The present invention is described below by specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.
[0053] Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.
[0054] In the following embodiments, the meanings of the abbreviations are as follows: HBP-NH2: amino-terminated hyperbranched polymer; CNF: carbon nanofiber; CNF-COOH: carbon nanofibers with carboxyl groups on the surface; CNF-NH2: carbon nanofibers with amino groups grafted on the surface; HATU: 2-(7-azabenzotriazole)-N,N,N',N'-tetramethyluronium hexafluorophosphate.
[0055] Example 1 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0056] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h and the xylene is added to the supergravity reactor at a flow rate of 70kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 100kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0057] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 60kg / h, and vinyltrichlorosilane was passed into the esterification reaction tower at a flow rate of 90kg / h. Vinyltrichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 100°C and the pressure to be -4kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyltrimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0058] In this embodiment, the platinum catalyst used in the preparation of vinyltrichlorosilane is prepared in the following steps: (1) Preparation of HBP-NH2: 4.0L triethylenetetramine and 8.0L methanol were mixed and placed in an ice bath. Under nitrogen protection, 2.4L methyl acrylate was slowly added dropwise while stirring. After the addition was completed, the mixture was stirred and reacted at room temperature (26°C) for 3.5h. Methanol was removed by vacuum rotary evaporation, and the temperature was raised to 110°C. The mixture was stirred and reacted at this temperature for 2.5h to obtain HBP-NH2.
[0059] (2) Preparation of CNF-COOH: 1.5 kg of CNF with a diameter of 50-100 nm and a length of 30-50 μm was added to 75 L of 30 wt% nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 65° C. for 1.5 h, the supernatant was removed by centrifugation, washed with water until neutral, and dried to obtain CNF-COOH.
[0060] (3) Preparation of HBP-NH2 / CNF composites: Take 360g of HBP-NH2 prepared in step (1) and dissolve it in 4.0L water, then add 400g of HATU and fully dissolve it to prepare a mixed solution for use. Take 1.0kg of CNF-COOH prepared in step (2) and add it to 15L water. After ultrasonic dispersion for 10min, add the mixed solution, stir evenly, react at 85℃ for 5h, centrifuge to remove the supernatant, wash with water 3 times, and dry to obtain 1.32kg of HBP-NH2 / CNF composite, and the mass ratio between CNF and HBP-NH2 is calculated to be 1:0.34.
[0061] (4) Formation of catalytic active sites: 1.32 kg of HBP-NH2 / CNF composite prepared in step (3) was dispersed in 60 L of 3 wt% chloroplatinic acid aqueous solution, adsorbed for 6 h, centrifuged to remove the supernatant, washed with water 3 times, and dried to obtain a platinum catalyst.
[0062] Example 2 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 70kg / h and hydrogen chloride at 165nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride in the synthesis kettle for gas-solid phase reaction, the temperature in the synthesis kettle is controlled to be 290℃, the pressure is 0.6MPa. The reaction to obtain a crude product, the crude product is sent to the condensation system, the crude product is cooled by cooling water, -35℃ refrigerant deep cooling into the first distillation tower for distillation, dichlorosilane by-product is separated, and then into the second distillation tower for distillation, silicon tetrachloride by-product is separated, and trichlorosilane is obtained. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0063] (2) Preparation of vinyl trichlorosilane: Platinum catalyst is added to the supergravity reactor at a flow rate of 220g / h and xylene at a flow rate of 80kg / h. After the catalyst is dissolved, dried acetylene gas is introduced at a flow rate of 35kg / h to activate the catalyst, and trichlorosilane is added at a flow rate of 90kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 100°C and the pressure is 100kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0064] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 80kg / h, and vinyltrichlorosilane was passed into the esterification reaction tower at a flow rate of 105kg / h. Vinyltrichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 110°C and the pressure to be -6kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyltrimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0065] In this embodiment, the platinum catalyst used in the preparation of vinyltrichlorosilane is prepared in the following steps: (1) Preparation of HBP-NH2: 4.0L triethylenetetramine and 8.0L methanol were mixed and placed in an ice bath. Under nitrogen protection, 2.0L methyl acrylate was slowly added dropwise while stirring. After the addition was completed, the mixture was stirred and reacted at room temperature (25°C) for 3h. Methanol was removed by vacuum rotary evaporation, and the temperature was raised to 100°C. The mixture was stirred and reacted at this temperature for 3h to obtain HBP-NH2.
[0066] (2) Preparation of CNF-COOH: 1.5 kg of CNF with a diameter of 50-100 nm and a length of 30-50 μm was added to 60 L of 30 wt% nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 60° C. for 2 h, the supernatant was removed by centrifugation, the mixture was washed with water until neutral, and dried to obtain CNF-COOH.
[0067] (3) Preparation of HBP-NH2 / CNF composites: Take 230g of HBP-NH2 prepared in step (1) and dissolve it in 2.5L water, then add 350g of HATU and fully dissolve it to prepare a mixed solution for use. Take 1.0kg of CNF-COOH prepared in step (2) and add it to 10L water. After ultrasonic dispersion for 10min, add the mixed solution, stir evenly, react at 80℃ for 6h, centrifuge to remove the supernatant, wash with water 3 times, and dry to obtain 1.2kg of HBP-NH2 / CNF composite, and the mass ratio between CNF and HBP-NH2 is calculated to be 1:0.21.
[0068] (4) Formation of catalytic active sites: 1.2 kg of HBP-NH2 / CNF composite prepared in step (3) was dispersed in 50 L of 5 wt% chloroplatinic acid aqueous solution, adsorbed for 12 h, centrifuged to remove the supernatant, washed with water three times, and dried to obtain a platinum catalyst.
[0069] Example 3 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 80kg / h and hydrogen chloride at 200nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride in the synthesis kettle for gas-solid phase reaction, the temperature in the synthesis kettle is controlled at 310℃, the pressure is 0.7MPa. The reaction to obtain a crude product, the crude product is sent to the condensation system, the crude product is cooled by cooling water, -35℃ refrigerant deep cooling into the first distillation tower for distillation, dichlorosilane by-product is separated, and then into the second distillation tower for distillation, silicon tetrachloride by-product is separated, and trichlorosilane is obtained. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0070] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 250g / h and the xylene is added to the supergravity reactor at a flow rate of 100kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 40kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 110kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 120°C and the pressure is 80kPa. The crude product obtained by the reaction is stored in a crude product tank, the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0071] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 100 kg / h, and vinyl trichlorosilane was passed into the esterification reaction tower at a flow rate of 130 kg / h. Vinyl trichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 120°C and the pressure to be -8 kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyl trimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0072] In this embodiment, the platinum catalyst used in the preparation of vinyltrichlorosilane is prepared in the following steps: (1) Preparation of HBP-NH2: 4.0L triethylenetetramine and 8.0L methanol were mixed and placed in an ice bath. Under nitrogen protection, 2.9L methyl acrylate was slowly added dropwise while stirring. After the addition was completed, the mixture was stirred and reacted at room temperature (25°C) for 4h. Methanol was removed by vacuum rotary evaporation, and the temperature was raised to 110°C. The mixture was stirred and reacted at this temperature for 2h to obtain HBP-NH2.
[0073] (2) Preparation of CNF-COOH: 1.5 kg of CNF with a diameter of 50-100 nm and a length of 30-50 μm was added to 90 L of 35 wt% nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 70° C. for 1 h, the supernatant was removed by centrifugation, the mixture was washed with water until neutral, and dried to obtain CNF-COOH.
[0074] (3) Preparation of HBP-NH2 / CNF composites: Take 450g of HBP-NH2 prepared in step (1) and dissolve it in 5L of water, then add 600g of HATU and fully dissolve it to prepare a mixed solution for use. Take 1.0kg of CNF-COOH prepared in step (2) and add it to 10L of water. After ultrasonic dispersion for 10min, add the mixed solution, stir evenly, react at 90℃ for 4h, centrifuge to remove the supernatant, wash with water 3 times, and dry to obtain 1.38kg of HBP-NH2 / CNF composite, and the mass ratio between CNF and HBP-NH2 is calculated to be 1:0.40.
[0075] (4) Formation of catalytic active sites: 1.38 kg of HBP-NH2 / CNF composite prepared in step (3) was dispersed in 70 L of 1 wt% chloroplatinic acid aqueous solution, adsorbed for 12 h, centrifuged to remove the supernatant, washed with water three times, and dried to obtain a platinum catalyst.
[0076] Example 4 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0077] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h and the xylene is added to the supergravity reactor at a flow rate of 70kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 100kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0078] (3) Formation of vinyl silane coupling agent: Ethanol was added to the vaporizer for vaporization, and then passed into the esterification tower at a flow rate of 60 kg / h, and vinyl trichlorosilane was passed into the esterification tower at a flow rate of 90 kg / h. Vinyl trichlorosilane and ethanol were subjected to esterification reaction in the esterification tower, and the temperature in the esterification tower was controlled to be 100°C and the pressure to be -4 kPa. The reaction obtained a crude product, part of which was refluxed to the esterification tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyl triethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification tower to react with ethanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0079] In this embodiment, the steps for preparing the platinum catalyst used in the preparation of vinyltrichlorosilane are the same as those in Embodiment 1.
[0080] Example 5 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0081] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h and the xylene is added to the supergravity reactor at a flow rate of 70kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 100kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0082] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification tower at a flow rate of 60 kg / h, and vinyl trichlorosilane was passed into the esterification tower at a flow rate of 90 kg / h. Vinyl trichlorosilane and methanol were subjected to esterification reaction in the esterification tower, and the temperature in the esterification tower was controlled to be 100°C and the pressure to be -4 kPa. The reaction obtained a crude product, part of which was refluxed to the esterification tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyl triethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0083] In this embodiment, the platinum catalyst used in the preparation of vinyltrichlorosilane is prepared in the following steps: (1) Preparation of HBP-NH2: 4.0L triethylenetetramine and 8.0L methanol were mixed and placed in an ice bath. Under nitrogen protection, 2.0L methyl acrylate was slowly added dropwise while stirring. After the addition was completed, the mixture was stirred and reacted at room temperature (25°C) for 3h. Methanol was removed by vacuum rotary evaporation, and the temperature was raised to 100°C. The mixture was stirred and reacted at this temperature for 3h to obtain HBP-NH2.
[0084] (2) Preparation of CNF-COOH: 1.5 kg of CNF with a diameter of 50-100 nm and a length of 30-50 μm was added to 60 L of 30 wt% nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 60° C. for 2 h, the supernatant was removed by centrifugation, the mixture was washed with water until neutral, and dried to obtain CNF-COOH.
[0085] (3) Preparation of HBP-NH2 / CNF composites: Take 130g of HBP-NH2 prepared in step (1) and dissolve it in 2.5L water, then add 350g of HATU and fully dissolve it to prepare a mixed solution for use. Take 1.0kg of CNF-COOH prepared in step (2) and add it to 10L water. After ultrasonic dispersion for 10min, add the mixed solution, stir evenly, react at 80℃ for 6h, centrifuge to remove the supernatant, wash with water 3 times, and dry to obtain 1.11kg of HBP-NH2 / CNF composite, and the mass ratio between CNF and HBP-NH2 is calculated to be 1:0.12.
[0086] (4) Formation of catalytic active sites: 1.11 kg of HBP-NH2 / CNF composite prepared in step (3) was dispersed in 46 L of 5 wt% chloroplatinic acid aqueous solution, adsorbed for 12 h, centrifuged to remove the supernatant, washed with water three times, and dried to obtain a platinum catalyst.
[0087] Example 6 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0088] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h and the xylene is added to the supergravity reactor at a flow rate of 70kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 100kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0089] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 60kg / h, and vinyltrichlorosilane was passed into the esterification reaction tower at a flow rate of 90kg / h. Vinyltrichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 100°C and the pressure to be -4kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyltrimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0090] In this embodiment, the platinum catalyst used in the preparation of vinyltrichlorosilane is prepared in the following steps: (1) Preparation of HBP-NH2: 4.0L triethylenetetramine and 8.0L methanol were mixed and placed in an ice bath. Under nitrogen protection, 2.9L methyl acrylate was slowly added dropwise while stirring. After the addition was completed, the mixture was stirred and reacted at room temperature (25°C) for 4h. Methanol was removed by vacuum rotary evaporation, and the temperature was raised to 110°C. The mixture was stirred and reacted at this temperature for 2h to obtain HBP-NH2.
[0091] (2) Preparation of CNF-COOH: 1.5 kg of CNF with a diameter of 50-100 nm and a length of 30-50 μm was added to 90 L of 35 wt% nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 70° C. for 1 h, the supernatant was removed by centrifugation, the mixture was washed with water until neutral, and dried to obtain CNF-COOH.
[0092] (3) Preparation of HBP-NH2 / CNF composites: Take 800g of HBP-NH2 prepared in step (1) and dissolve it in 5.0L water, then add 600g of HATU and fully dissolve it to prepare a mixed solution for use. Take 1.0kg of CNF-COOH prepared in step (2) and add it to 100mL of water. After ultrasonic dispersion for 10min, add the mixed solution, stir evenly, react at 90℃ for 4h, centrifuge to remove the supernatant, wash with water 3 times, and dry to obtain 1.69kg of HBP-NH2 / CNF composite, and the mass ratio between CNF and HBP-NH2 is calculated to be 1:0.71.
[0093] (4) Formation of catalytic active sites: 1.69 kg of HBP-NH2 / CNF composite prepared in step (3) was dispersed in 85.5 L of 1 wt% chloroplatinic acid aqueous solution, adsorbed for 12 h, centrifuged to remove the supernatant, washed with water three times, and dried to obtain a platinum catalyst.
[0094] Comparative Example 1 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0095] (2) Preparation of vinyl trichlorosilane: The platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h and the xylene is added to the supergravity reactor at a flow rate of 70kg / h. After the catalyst is dissolved, the dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and then trichlorosilane is added at a flow rate of 100kg / h. The materials are mixed evenly, and acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor. The temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned, filtered and separated, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0096] (3) Formation of vinyl silane coupling agent: Methanol is added to the vaporizer for vaporization, and then passed into the esterification tower at a flow rate of 60kg / h, and vinyltrichlorosilane is passed into the esterification tower at a flow rate of 90kg / h. Vinyltrichlorosilane and methanol are subjected to esterification reaction in the esterification tower, and the temperature in the esterification tower is controlled to be 100°C and the pressure is -4kPa. The reaction obtains a crude product, part of which is refluxed to the esterification tower through a material reflux pump, and part of the crude product is sent to a neutralization kettle for neutralization with sodium alcohol. The crude product after neutralization enters two distillation towers for distillation, and the obtained vinyltrimethoxysilane is stored in a finished product tank. The by-product separated by distillation returns to the esterification tower to react with methanol again. The hydrogen chloride gas generated during the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, it enters two stages of condensation, demisting, and distillation, and then is reused in the synthesis kettle to react with silicon powder.
[0097] In this comparative example, the steps for preparing the platinum catalyst used in the preparation of vinyltrichlorosilane are the same as those in Example 1.
[0098] Comparative Example 2 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0099] (2) Preparation of vinyl trichlorosilane: Activated carbon-supported chloroplatinic acid is used as a catalyst. The catalyst is added to the supergravity reactor at a flow rate of 200g / h and xylene at a flow rate of 70kg / h. After the catalyst is dissolved, dried acetylene gas is introduced at a flow rate of 30kg / h to activate the catalyst, and trichlorosilane is added at a flow rate of 100kg / h. The materials are evenly mixed, acetylene and trichlorosilane are subjected to hydrogen silane addition reaction in the supergravity reactor, and the temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, and the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned and filtered to separate, and it is used again to catalyze the hydrosilane addition reaction. The gas generated by the hydrogen silane addition reaction is condensed to the tail gas recovery tank through two stages, part of which is introduced into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0100] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 60kg / h, and vinyltrichlorosilane was passed into the esterification reaction tower at a flow rate of 90kg / h. Vinyltrichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 100°C and the pressure to be -4kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyltrimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0101] In this comparative example, the activated carbon-supported chloroplatinic acid catalyst used in the preparation of vinyltrichlorosilane was prepared in the following steps: (1) Preparation of AC-COOH: 1.5 kg AC was added into 75 L 30 wt % nitric acid solution, and after ultrasonic dispersion for 10 min, the mixture was stirred and reacted at 65° C. for 1.5 h, and the supernatant was removed by centrifugation. The mixture was washed with water until neutral, and dried to obtain AC-COOH.
[0102] (2) Preparation of AC-NH2: Take 360g of ethylenediamine and 4.0L of water, mix them, then add 400g of HATU and fully dissolve them to prepare a mixed solution for use. Take 1.0kg of AC-COOH prepared in step (1), add it to 50L of water, ultrasonically disperse it for 10min, add the mixed solution, stir it evenly, react it at 85℃ for 5h, centrifuge to remove the supernatant, wash it with water 3 times, and dry it to obtain AC-NH2.
[0103] (3) Formation of catalytic active sites: The AC-NH2 prepared in step (2) was dispersed in 60 L of 3 wt% chloroplatinic acid aqueous solution, adsorbed for 6 h, centrifuged to remove the supernatant, washed with water 3 times, and dried to obtain an activated carbon-supported chloroplatinic acid catalyst.
[0104] Comparative Example 3 A vinyl silane coupling agent is prepared by the following steps: (1) Preparation of trichlorosilane: After adding the silicon powder into the dryer, dry it with dry nitrogen at 160°C for 4 hours, and then dry the dried silicon powder at a flow rate of 60kg / h and hydrogen chloride at 140nm. 3 / h flow rate into the synthesis kettle, silicon powder and hydrogen chloride react in the synthesis kettle in the gas-solid phase, the temperature in the synthesis kettle is controlled to be 280℃, and the pressure is 0.7MPa. The reaction obtains a crude product, which is sent to the condensation system. The crude product is cooled by cooling water, deep cooled by -35℃ refrigerant, and then enters the first distillation tower for distillation to separate the dichlorosilane by-product, and then enters the second distillation tower for distillation to separate the tetrachlorosilane by-product to obtain trichlorosilane. The hydrogen generated in the reaction process is extracted by pressure swing adsorption equipment.
[0105] (2) Preparation of vinyl trichlorosilane: Platinum catalyst is added to the supergravity reactor at a flow rate of 200g / h, xylene at a flow rate of 70kg / h, dried acetylene gas at a flow rate of 30kg / h, and trichlorosilane at a flow rate of 100kg / h. The materials are mixed evenly, acetylene and trichlorosilane are subjected to hydrogen silicon addition reaction in the supergravity reactor, and the temperature in the supergravity reactor is controlled to be 80°C and the pressure is 120kPa. The crude product obtained by the reaction is stored in a crude product tank, the platinum catalyst is first filtered and separated, and then distilled through 6 distillation towers to remove 1,2-bis(trichlorosilyl)ethane to obtain vinyl trichlorosilane. The platinum catalyst is cleaned and filtered to separate, and it is used again to catalyze the hydrosilylation reaction. The gas produced by the hydrogen silicon addition reaction is condensed to the tail gas recovery tank through two stages, part of which is passed into the supergravity reactor for further reaction, and part of which enters the tail gas absorption system through the venting condenser.
[0106] (3) Formation of vinyl silane coupling agent: Methanol was added to the vaporizer for vaporization, and then passed into the esterification reaction tower at a flow rate of 60kg / h, and vinyltrichlorosilane was passed into the esterification reaction tower at a flow rate of 90kg / h. Vinyltrichlorosilane and methanol were subjected to esterification reaction in the esterification reaction tower, and the temperature in the esterification reaction tower was controlled to be 100°C and the pressure to be -4kPa. The reaction obtained a crude product, part of which was refluxed to the esterification reaction tower through a material reflux pump, and part of which was sent to a neutralization kettle for neutralization with sodium alcoholate. The neutralized crude product entered two distillation towers for distillation, and the obtained vinyltrimethoxysilane was stored in a finished product tank, and the by-product separated by distillation was returned to the esterification reaction tower to react with methanol again. The hydrogen chloride gas produced in the esterification reaction flows out from the top of the tower, and after standing in a pressure vessel, enters an ultra-gravity reactor, and is washed with silicon tetrachloride filtered through a microporous filter. The silicon tetrachloride is a by-product produced in the preparation of trichlorosilane. After two stages of condensation, demisting and distillation, high-purity hydrogen chloride is obtained, and the hydrogen chloride is recycled to the synthesis kettle to react with silicon powder.
[0107] In this comparative example, the steps for preparing the platinum catalyst used in the preparation of vinyltrichlorosilane are the same as those in Example 1.
[0108] Test Example 1 The trichlorosilane prepared according to the methods in Example 1 and Comparative Example 1 was subjected to gas chromatography analysis, and its selectivity and yield were calculated. The results are shown in Table 1.
[0109] Table 1 Trichlorosilane test results Selectivity / % Yield / % Example 1 99.2 98.7 Comparative Example 1 94.5 93.2 From Table 1 we can see that: The selectivity and yield of Example 1 are significantly higher than those of Comparative Example 1. This is because, in Example 1, the distillation residue of hydrogen chloride is subjected to a washing treatment, so that the recycled hydrogen chloride contains a small amount of silicon tetrachloride, which can inhibit the occurrence of side reactions in the trichlorosilane preparation process, and at the same time can realize the recycling of the reaction by-products, thereby improving the selectivity and yield of trichlorosilane.
[0110] Test Example 2 The vinyltrimethoxysilane or vinyltriethoxysilane prepared according to the methods in the examples and comparative examples was subjected to gas chromatography analysis, and its selectivity and yield were calculated. The results are shown in Table 2.
[0111] Table 2 Test results of vinyl trimethoxysilane or vinyl triethoxysilane Selectivity / % Yield / % Example 1 99.3 98.8 Example 2 98.9 98.5 Example 3 99.5 99.2 Example 4 98.6 98.5 Example 5 95.7 95.4 Example 6 96.6 96.4 Comparative Example 2 86.8 86.1 From Table 2 we can see that: (1) In Examples 1 to 6, the selectivity of the prepared vinyltrimethoxysilane and vinyltriethoxysilane can reach more than 95.7%, and the yield can reach more than 95.4%, indicating that the method for preparing the vinyl silane coupling agent can achieve higher reaction selectivity and product yield.
[0112] (2) The selectivity of Example 2 is higher than that of Example 5, and the selectivity of Example 3 is higher than that of Example 6, indicating that the reaction selectivity can be improved to a greater extent by controlling the mass ratio of CNF and HBP-NH2 in the platinum catalyst to 1:0.2-0.4.
[0113] (3) The selectivity and yield of Example 1 are significantly higher than those of Comparative Example 2. This is because the catalyst selected in Example 1 uses a composite network of HBP-NH2 and CNF to load platinum elements, wherein the heat-conducting network composed of CNF can achieve rapid heat dissipation during the reaction, thereby reducing the generation of by-products and improving the reaction selectivity; while in Comparative Example 2, activated carbon is used to load chloroplatinic acid. Due to the presence of a large number of closed-pore structures inside the activated carbon, the thermal conductivity is poor, and the heat released in the hydrosilylation reaction will cause the local temperature to be too high, thereby causing the side reactions to intensify.
[0114] Test Example 3 The vinyltrichlorosilane prepared according to the methods in Example 1 and Comparative Example 3 was analyzed by gas chromatography to calculate the reaction time and selectivity required for a conversion rate of 98%. The results are shown in Table 3.
[0115] Table 3 Vinyl trichlorosilane test results Reaction time (h) Selectivity% Example 1 4.3 99.1 Comparative Example 3 5.1 98.5 From Table 3 we can see that: Compared with Comparative Example 3, Example 1 has a shorter reaction time and higher selectivity. This indicates that pre-activating the catalyst before subjecting it to the hydrosilylation reaction can shorten the reaction time and improve the reaction selectivity.
[0116] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0117] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a vinyl silane coupling agent, characterized in that: The following steps are involved: S1: reacting silicon powder with hydrogen chloride, and subjecting the product to purification treatment including distillation to obtain trichlorosilane and a distillation residue containing silicon tetrachloride; S2: pre-activating the catalyst, reacting trichlorosilane with acetylene under the action of the activated catalyst and an inert solvent, separating and purifying the product to obtain vinyl trichlorosilane; S3: reacting vinyltrichlorosilane with alcohol, separating and purifying the product to obtain a vinylsilane coupling agent, recovering the hydrogen chloride gas generated during the reaction, and recycling the hydrogen chloride gas to step S1 after purification treatment including washing with distillation residue containing silicon tetrachloride.
2. The method for preparing a vinyl silane coupling agent according to claim 1, characterized in that: The catalyst used in S2 is a platinum catalyst; the platinum catalyst includes a composite network composed of mutually cross-linked carbon nanofibers and amino-terminated hyperbranched polymers, and a platinum element bound to the amino-terminated hyperbranched polymer; the amino-terminated hyperbranched polymer is covalently bonded to the surface of the carbon nanofibers through amide bonds, so that connections are formed between the carbon nanofibers.
3. A method for preparing a vinyl silane coupling agent according to claim 1 or 2, characterized in that: The inert solvent used in S2 is xylene.
4. The method for preparing a vinyl silane coupling agent according to claim 1, characterized in that: The silicon powder and hydrogen chloride in S1 react in a reactor, the silicon powder at a flow rate of 60-80 kg / h, and the hydrogen chloride at a flow rate of 140-200 nm. 3 / h was added to the reactor.
5. The method for preparing a vinyl silane coupling agent according to claim 4, characterized in that: The reaction temperature of the reactor in S1 is 280-310° C., and the reaction pressure is 0.5-0.7 MPa.
6. The method for preparing a vinyl silane coupling agent according to claim 1, characterized in that: In S1, a pressure swing adsorption device is used to extract the hydrogen generated by the reaction.
7. The method for preparing a vinyl silane coupling agent according to claim 1, characterized in that: The acetylene and trichlorosilane in S2 react in a reactor, and acetylene is added to the reactor at a flow rate of 30-40 kg / h, and trichlorosilane is added to the reactor at a flow rate of 75-110 kg / h.
8. The method for preparing a vinyl silane coupling agent according to claim 7, characterized in that: The reaction temperature of the reactor in S2 is 80-120° C., and the reaction pressure is 80-120 kPa.
9. The method for preparing a vinyl silane coupling agent according to claim 1, characterized in that: In S3, vinyltrichlorosilane and alcohol react in a reactor, and vinyltrichlorosilane is added to the reactor at a flow rate of 90 to 130 kg / h, and alcohol is added to the reactor at a flow rate of 60 to 100 kg / h.
10. The method for preparing a vinyl silane coupling agent according to claim 9, characterized in that: The reaction temperature of the reactor in S3 is 100 to 120° C., and the reaction pressure is -8 to -4 kPa.