Water-soluble polyester as well as preparation method and application thereof

By adjusting the raw material components and reaction conditions of water-soluble polyester in the environmentally friendly catalyst reaction system, the problems of self-polymerization of monomers and high heavy metal content are solved, and the stability and uniformity of water-soluble polyester are achieved, ensuring marine islands The uniform phase distribution and fast fiber opening speed reduce heavy metal content, improve processing performance and environmental protection.

CN118894983AActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310491783.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-05
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

During the polycondensation process of existing water-soluble polyesters, the monomers are prone to self-polymerization, and the glass transition temperature and crystallization degree are too low, resulting in unstable pressure during spinning, uneven distribution of marine island phases, uneven fiber opening, and heavy metals. High content affects the environment and product quality.

Method used

In a specific environmentally friendly catalyst reaction system, water-soluble polyester with intrinsic viscosity and shear viscosity within a specific range is prepared by adjusting the proportion of raw material components and reaction conditions to ensure its stability and uniformity at high shear rates. and the polymerization reaction is controlled by titanium catalyst to reduce the heavy metal content.

Benefits of technology

The stability and uniformity of water-soluble polyester are achieved, ensuring uniform distribution of marine island phases, fast and stable fiber opening speed, reducing heavy metal content, and improving processing performance and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894983A_ABST
    Figure CN118894983A_ABST
Patent Text Reader

Abstract

The invention relates to the field of polymer chemical industry, and discloses water-soluble polyester as well as a preparation method and application thereof. The intrinsic viscosity of the water-soluble polyester is 0.50-0.55 dL / g, and the shear viscosity of the water-soluble polyester is 50-60 Pa.s under the conditions that the temperature is 288 DEG C and the shear rate is 6000 s <-1 >; the preparation method of the water-soluble polyester comprises the following steps: in the presence of a titanium catalyst, carrying out a reaction I on a binary acid monomer and a dihydric alcohol monomer to obtain a reactant I; and carrying out a reaction II on the reactant I, bis (2-hydroxyethyl) isophthalate-5-sodium sulfonate and polyethylene glycol. The water-soluble polyester has specific intrinsic viscosity and shear viscosity, and can effectively ensure the distribution uniformity of a sea phase and an island phase when being applied to the preparation process of the sea-island fiber, so that the purposes of uniform distribution of the sea phase and the island phase in the fiber and high and stable splitting speed are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer chemical industry, and in particular to a water-soluble polyester and a preparation method and application thereof. Background Art

[0002] The domestic polyester production capacity has increased year by year, and conventional polyester and fiber have shown a trend of oversupply. The development of functional polyester has become an important measure to expand the use of polyester and improve the level of differentiation. Water-soluble polyester (COPET) is a polyester that can be dissolved in hot water (alkaline) by adding modified components during the polyester synthesis process. At present, water-soluble polyester chips are mainly used in the production of sea-island composite ultrafine fibers. Other applications include microporous, dry fibers, improved dyeing fibers, and fabric alkali reduction treatment.

[0003] In the field of spinning, water-soluble polyester is mainly used as the dissolving component of chemical fiber ultrafine composite spinning. Compared with mechanical stripping and solvent stripping, this water-soluble stripping method has obvious advantages and can obtain finer and more uniform ultrafine fibers. Compared with the solvent stripping method, it can avoid the disadvantages of using various toxic and environmentally polluting solvents, and only hot alkali solution is needed to achieve stripping, which is conducive to industrial implementation and environmental protection requirements. The ultrafine denier fiber prepared by water-soluble polyester has the advantages of soft hand feel, good smoothness, moisture absorption and perspiration, high strength, etc., so it is widely used in the fields of imitation leather, high-end fabrics, sportswear, special drawing paper, etc.

[0004] In order to prepare polyester with water-soluble properties, relevant research has been conducted on the preparation process and raw materials of polyester. Many patents focus on the formulation research of water-soluble polyester. For example, the water-soluble polyesters disclosed in CN107602832A and CN106674508A are made of functional raw materials such as terephthalic acid (PTA), isophthalic acid (IPA), ethylene glycol (EG), sodium isophthalate-5-sulfonate (SIPE), polyethylene glycol (PEG), etc.; CN105669959A uses itaconic acid and its sulfonated product sodium itaconic acid sulfonate instead of traditional Hydrophilic monomers and dibasic acids containing benzene rings are added with 1,4-butanediol, and a new type of water-soluble polyester (PBIINa) is synthesized by direct esterification polycondensation; CN104371096A uses terephthalic acid, ethylene glycol, neopentyl glycol, polyethylene glycol, sodium 5-sulfonate of ethylene isophthalate and aliphatic dibasic acids as monomers, antimony trioxide or antimony acetate as catalysts, trimethyl phosphate as stabilizer, and obtains water-soluble polyester through esterification process, polymerization process and post-treatment unit process. Although these patents have studied the formula of water-soluble polyester, the research scope of monomers is wide, resulting in large differences in thermal properties and water solubility of subsequent water-soluble polyesters, which affects the stability of spinning process and fiber opening process in actual application, and may further lead to uneven separation of sea phase and island phase in sea island yarn after alkali dissolution fiber opening. In addition, CN1438274A and CN101407946A respectively add 4-8 mol % of isophthalic acid (IPA) or 11-20 mol % of isophthalic acid during the polymerization process of producing water-soluble polyester. The addition of such a high content of IPA will lead to the deterioration of the crystallization performance of the water-soluble polyester, affect the processing process of the sea island silk, and cause abnormal phenomena such as defects and breakage.

[0005] In order to reduce heavy metal pollution in the fiber opening process, CN103130996A discloses an alkali-soluble polyester and a preparation method thereof, wherein the polyester contains repeating units synthesized from terephthalic acid and ethylene glycol, wherein the content of sodium dimethyl isophthalate-5-sulfonate is equivalent to 2-8 mol% of the total dibasic acid units, and the content of metal elements other than sodium in the polyester is below 3 ppm; sodium dimethyl isophthalate-5-sulfonate, a catalyst organic sulfonic acid and a regulator organic amine compound are added in the polycondensation stage, and the polycondensation temperature is too high, and SIPE self-polymerization may occur in the actual production process, thereby causing the problem of violent polymerization of the polymer.

[0006] In summary, although after years of development, water-soluble polyester as a soluble component for island fiber composite spinning has a mature set of synthesis, spinning, weaving, fiber opening, dyeing and finishing technologies, but due to its high difficulty in polymerization and strict requirements on spinning conditions, it has not yet formed a unified product standard. Therefore, in the actual production process, there are abnormal phenomena such as drying and bonding, uneven fiber opening, etc. In order to overcome these problems, water-soluble polyester needs to meet the following four requirements: (1) From the perspective of reaction process, the key to the process of water-soluble polyester is to select appropriate catalysts and functional monomers to make the polycondensation reaction stable and prevent the rapid polymerization of monomers; (2) For the performance of water-soluble polyester, it is necessary to ensure that there is a suitable glass transition temperature and crystallization rate to prevent the water-soluble polyester from bonding and poor fiber performance during use; (3) In the process of island fiber forming, it is necessary to ensure that the box pressure of water-soluble polyester and conventional polyester is similar, and the spinning island phase structure is uniform; (4) The fiber opening process is fast and stable, and the pollution of process wastewater to the environment is reduced as much as possible.

[0007] Therefore, based on the current research status of water-soluble polyesters, the development of water-soluble polyesters with smooth polycondensation reaction, crystallization properties not much different from conventional polyesters, low heavy metal content, easy solubility in alkaline water and steady rate has certain market prospects and environmental benefits. Summary of the invention

[0008] The purpose of the present invention is to overcome a series of technical difficulties existing in the prior art, such as the monomers are easy to self-polymerize during the polycondensation process of water-soluble polyester, the glass transition temperature and crystallinity are too low, which makes the slices easy to stick together, the pressure is unstable during the spinning process, resulting in uneven distribution of the sea phase island phase, and the fiber opening cannot be guaranteed to be uniform and stable, and to provide a water-soluble polyester and its preparation method and application.

[0009] The inventors of the present invention unexpectedly discovered in their research that in a specific environmentally friendly catalyst reaction system, by matching the dosage of each raw material component, the reaction conditions and the content of a specific component in the obtained water-soluble polyester, the obtained water-soluble polyester has stable water solubility, crystallization and processing performance, while strictly controlling the characteristic viscosity and shear viscosity of the water-soluble polyester within a specific range, which can effectively ensure the formation of a stable sea island phase distribution in the process of sea island yarn forming, and improve the uniformity of the sea phase distribution in the fiber and the fiber opening speed. The inventors further found in their research that at a temperature of 288°C and a shear rate of 6000s -1 The shear viscosity under the conditions of 6000s / s and the shear viscosity under the conditions of 6000s / s when the water-soluble polyester is used to produce the sea-island fiber. -1Under the above conditions, the shear viscosity ratio between the water-soluble polyester and the conventional polyester used in the island phase can be used as a key control indicator of the water-soluble polyester to ensure the uniformity of the sea phase and island phase structure in the subsequent sea island yarn forming process, and the fiber opening speed is fast and stable. Based on the above findings, the present invention is proposed.

[0010] In order to achieve the above object, the present invention provides a water-soluble polyester in the first aspect, wherein the intrinsic viscosity of the water-soluble polyester is 0.50-0.55 dL / g, and the water-soluble polyester has a temperature of 288°C and a shear rate of 6000s -1 The shear viscosity under the conditions is 50-60Pa·s.

[0011] A second aspect of the present invention provides a method for preparing a water-soluble polyester, the method comprising the following steps:

[0012] (1) reacting a dibasic acid monomer with a diol monomer in the presence of a titanium catalyst to obtain a reactant I;

[0013] (2) reacting the reactant I with sodium bis(hydroxyethyl)-5-sulfonate isophthalate and polyethylene glycol to react II;

[0014] Among them, based on the total amount of the dibasic acid monomer and the diol monomer as 100 parts by weight, the amount of the titanium-based catalyst is 0.0015-0.003 parts by weight, the amount of sodium bis(hydroxyethyl)isophthalate-5-sulfonate is 4.5-7 parts by weight, and the amount of polyethylene glycol is 4.5-7 parts by weight.

[0015] The third aspect of the present invention provides the use of the above-mentioned water-soluble polyester and the water-soluble polyester prepared by the above-mentioned method in the production of chemical fibers.

[0016] The fourth aspect of the present invention provides a method for producing sea-island fibers, the method comprising the following steps: using the above-mentioned water-soluble polyester and / or the water-soluble polyester prepared by the above-mentioned method as the sea phase and using conventional polyester as the island phase; wherein, at a temperature of 288°C and a shear rate of 6000s -1 Under the conditions, the shear viscosity ratio of the water-soluble polyester to the conventional polyester is 0.8-0.9:1.

[0017] The water-soluble polyester provided by the present invention is an environmentally friendly polyester that is quickly soluble in water and has specific intrinsic viscosity and shear viscosity. When applied to a spinning process, it can form a specific shear viscosity ratio with conventional polyester, effectively ensuring the uniformity of the distribution of the sea phase (the water-soluble polyester provided by the present invention) and the island phase (conventional polyester), thereby achieving the purpose of uniform distribution of the sea phase and the island phase in the fiber and fast and stable fiber opening speed; further, the glass transition temperature and semi-crystallization period of the water-soluble polyester provided by the present invention are close to those of conventional polyester, the processing performance is good, and the water solubility is significantly better than that of conventional polyester, and the heavy metal content is significantly reduced.

[0018] In the preparation method of the water-soluble polyester provided by the invention, the polycondensation reaction is stable and the drying process is simple, and the method is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a cross-sectional view of the sea island phase of the sea island precursor when the water-soluble polyester prepared in Example 1 is used as the sea phase;

[0020] Figure 2 This is a cross-sectional view of the sea island phase of the sea island precursor when the polyester prepared in Comparative Example 2 is used as the sea phase;

[0021] Figure 3 This is a microscopic morphology of the garter after alkali reduction treatment when the water-soluble polyester prepared in Example 1 is used as the sea phase;

[0022] Figure 4 This is a microscopic morphology of the garter after alkali reduction treatment when the polyester prepared in Example 2 is used as the sea phase. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] The first aspect of the present invention provides a water-soluble polyester having an intrinsic viscosity of 0.50-0.55 dL / g and a shear rate of 6000 s at a temperature of 288°C. -1 The shear viscosity under the conditions is 50-60Pa·s.

[0025] In the present invention, the intrinsic viscosity is tested and characterized according to 5.1 of GB / T14190-2017 Test Method for Fiber-Grade Polyester Chips; the shear viscosity is obtained by testing the rheological properties of the sample using a capillary rheometer, wherein the capillary die diameter is 1 mm, the aspect ratio L / D=16, the inlet angle is 90°, the test temperature is 288°C, and the shear rate is 6000s -1 .

[0026] The water-soluble polyester provided by the present invention has specific characteristic viscosity and shear viscosity. When applied to the sea-island yarn forming process, it can effectively ensure that the water-soluble polyester forms a stable sea-island phase distribution, thereby improving the uniformity of sea-island phase distribution in the fiber and the fiber opening speed.

[0027] According to the present invention, preferably, the intrinsic viscosity of the water-soluble polyester is 0.515-0.53 dL / g, at a temperature of 288°C and a shear rate of 6000s -1 The shear viscosity under the conditions is 52-58.5 Pa·s.

[0028] In order to realize the application of the water-soluble polyester provided by the present invention in the production of chemical fibers, especially sea-island fibers, the water-soluble polyester should have stable water solubility, crystallization performance and processing performance on the basis of having specific intrinsic viscosity and shear viscosity. Preferably, the glass transition temperature of the water-soluble polyester is 55-68°C, the half crystallization period is 2-4min, and the water solubility under the alkali reduction process conditions of temperature of 100°C, alkali content of 1wt%, and time of 45min is greater than or equal to 51.6%; the glass transition temperature and melt crystallization rate of the water-soluble polyester are close to those of conventional polyester, and the processing performance is good.

[0029] In the present invention, the glass transition temperature (Tg), the half crystallization period (t 1 / 2 ) was tested and calculated using differential scanning calorimetry (DSC). The specific process was as follows: under nitrogen protection, DSC thermal analysis was used to increase the temperature from 25°C to 290°C at a heating rate of 10°C / min, hold for 5 minutes, then cool down to 25°C at a rate of 400°C / min, then increase the temperature from 25°C to 290°C at a heating rate of 10°C / min, hold for 5 minutes, and finally cool down to 100°C at a rate of 10°C / min. The glass transition temperature Tg was calculated based on the second heating curve, and the crystallinity of the melt crystallization peak was used to calculate the half-crystallization period t in the melt crystallization process. 1 / 2 The alkali reduction process refers to the dissolution rate of the water-soluble polyester after the water-soluble polyester is treated in an alkali solution with a temperature of 100°C and an alkali content of 1wt% for 45 minutes.

[0030] According to the present invention, preferably, the water-soluble polyester contains sodium bis(hydroxyethyl)isophthalate-5-sulfonate units, polyethylene glycol units and titanium. The sodium bis(hydroxyethyl)isophthalate-5-sulfonate units refer to the groups formed after the esterification of sodium bis(hydroxyethyl)isophthalate-5-sulfonate; the polyethylene glycol units refer to the groups formed after the esterification of polyethylene glycol; and the titanium element comes from the titanium catalyst in the synthesis process of the water-soluble polyester.

[0031] According to the present invention, preferably, the polyethylene glycol unit is selected from at least one of PEG1500 unit, PEG2000 unit and PEG4000 unit; more preferably, it is PEG2000 unit.

[0032] In the present invention, the content of sodium bis(hydroxyethyl)isophthalate-5-sulfonate unit and polyethylene glycol unit in the water-soluble polyester can be obtained by nuclear magnetic resonance hydrogen spectrum (NMR), and the content of titanium element can be obtained by elemental analysis method. Preferably, the content of sodium bis(hydroxyethyl)isophthalate-5-sulfonate unit is 6-8wt%, the content of polyethylene glycol unit is 6-8wt%, and the content of titanium element is 0.0003-0.0005wt%. The inventors found that under this preferred embodiment, it is conducive to achieving the characteristics of low heavy metal content, rapid water solubility, good processing performance, stable and uniform fiber opening of the water-soluble polyester, and has significant functionalization and greening effects.

[0033] According to the present invention, the water-soluble polyester can be prepared by using a variety of raw material components to form a specific catalyst reaction system, so as to have the above-mentioned specific intrinsic viscosity, shear viscosity, and stable water solubility, crystallization performance and processing performance. Preferably, the raw material components of the water-soluble polyester contain dibasic acid monomers, diol monomers, sodium bis(hydroxyethyl)isophthalate-5-sulfonate, polyethylene glycol and titanium catalyst; wherein the titanium catalyst is used as a catalyst for the esterification reaction of the dibasic acid monomer and the diol monomer.

[0034] According to the present invention, preferably, the dibasic acid monomer can be selected from at least one of terephthalic acid, isophthalic acid and adipic acid; more preferably, terephthalic acid.

[0035] According to the present invention, preferably, the diol monomer is ethylene glycol and / or pentanediol; more preferably ethylene glycol.

[0036] According to the present invention, preferably, the polyethylene glycol is selected from at least one of PEG1500, PEG2000 and PEG4000; more preferably PEG2000.

[0037] According to the present invention, preferably, the titanium-based catalyst is tetrabutyl titanate and / or titanium glycol; more preferably, it is tetrabutyl titanate.

[0038] In the present invention, the above-mentioned dibasic acid monomer, diol monomer, sodium bis(hydroxyethyl)isophthalate-5-sulfonate, polyethylene glycol and titanium catalyst can be obtained commercially or prepared by the preparation method disclosed in the prior art.

[0039] A second aspect of the present invention provides a method for preparing a water-soluble polyester, the method comprising the following steps:

[0040] (1) reacting a dibasic acid monomer with a diol monomer in the presence of a titanium catalyst to obtain a reactant I;

[0041] (2) reacting the reactant I with sodium bis(hydroxyethyl)-5-sulfonate isophthalate and polyethylene glycol to react II;

[0042] Among them, based on the total amount of the dibasic acid monomer and the diol monomer as 100 parts by weight, the amount of the titanium-based catalyst is 0.0015-0.003 parts by weight, the amount of sodium bis(hydroxyethyl)isophthalate-5-sulfonate is 4.5-7 parts by weight, and the amount of polyethylene glycol is 4.5-7 parts by weight.

[0043] The preparation method of the water-soluble polyester of the present invention is simple and suitable for industrial production. By limiting the raw material dosage of titanium catalyst, sodium bis(hydroxyethyl)isophthalate-5-sulfonate (SIPE) and polyethylene glycol (PEG) in the preparation process of the water-soluble polyester, the contents of titanium element, SIPE unit and PEG unit in the water-soluble polyester are controlled, so that the content of sodium bis(hydroxyethyl)isophthalate-5-sulfonate unit (SIPE unit) in the water-soluble polyester is 6-8wt%, the content of polyethylene glycol unit (PEG unit) is 6-8wt%, and the content of titanium element is 0.0003-0.0005wt%. The intrinsic viscosity of the obtained water-soluble polyester is 0.5-0.55dL / g, and the water-soluble polyester is 0.0003-0.0005wt% at a temperature of 288°C and a shear rate of 6000s -1 The shear viscosity under the conditions is 50-60Pa·s.

[0044] According to the present invention, preferably, the intrinsic viscosity of the water-soluble polyester is 0.515-0.53 dL / g, and the water-soluble polyester has a temperature of 288°C and a shear rate of 6000 s -1 The shear viscosity under the conditions is 52-58.5 Pa·s.

[0045] According to the present invention, preferably, the glass transition temperature of the water-soluble polyester is 55-68°C, the half crystallization period is 2-4min, and the water solubility under the alkali reduction process conditions of temperature of 100°C, alkali content of 1wt% and time of 45min is greater than or equal to 51.6%.

[0046] According to the present invention, preferably, the dibasic acid monomer is selected from at least one of terephthalic acid, isophthalic acid and adipic acid; more preferably terephthalic acid.

[0047] According to the present invention, preferably, the diol monomer is ethylene glycol and / or pentanediol; more preferably ethylene glycol.

[0048] According to the present invention, preferably, the polyethylene glycol is selected from at least one of PEG1500, PEG2000 and PEG4000; more preferably PEG2000.

[0049] According to the present invention, preferably, the titanium-based catalyst is tetrabutyl titanate and / or titanium glycol; more preferably, it is tetrabutyl titanate.

[0050] According to the present invention, preferably, the weight ratio of the dibasic acid monomer to the diol monomer is 1-2.5:1; more preferably 1.5-1.9:1. The inventors found that under this preferred embodiment, it is beneficial to achieve stable water solubility, crystallization and processing performance of the water-soluble polyester, while limiting the intrinsic viscosity and shear viscosity within a specific range, so as to improve the uniformity of the distribution of the sea phase island phase in the fiber and the fiber opening speed.

[0051] According to the present invention, it is further preferred that the amounts of sodium bis(hydroxyethyl)isophthalate-5-sulfonate and polyethylene glycol in the water-soluble polyester are similar, and the raw material amount ratio of sodium bis(hydroxyethyl)isophthalate-5-sulfonate and polyethylene glycol in the preparation process of the water-soluble polyester is also preferably 0.79-1.26:1, and more preferably 0.95-1.05:1.

[0052] According to the present invention, preferably, the conditions of reaction I in step (1) at least include: temperature of 230-260°C, absolute pressure of 0.2-0.4 MPa, and time of 60-240 min. The inventors have found that under this preferred embodiment, it is beneficial to achieve stable water solubility, crystallization performance and processing performance of the water-soluble polyester, while limiting the intrinsic viscosity and shear viscosity within a specific range.

[0053] According to the present invention, preferably, the process of reaction II in step (2) includes: firstly performing a pre-polycondensation reaction and then performing a final polycondensation reaction. The inventors have found that under this preferred embodiment, the stability of the water-soluble polyester is improved.

[0054] According to the present invention, preferably, the conditions of the pre-polycondensation reaction at least include: heating reaction at a temperature range of 260-275°C, an absolute pressure of 0.1-100KPa, and a time of 40-50min. The inventors found that under this preferred embodiment, it is beneficial to combine the reaction process with the amount of each raw material, so that the prepared water-soluble hydrogel has a specific characteristic viscosity and shear viscosity, and the water-soluble polyester has the characteristics of rapid water solubility, good processing performance, and stable and uniform fiber opening.

[0055] According to the present invention, preferably, the conditions of the final polycondensation reaction include at least: a temperature of 270-285°C, an absolute pressure of less than 100Pa, and a time of 70-85min. The time of the final polycondensation reaction can be controlled by the cumulative time after the stirring current of the reactor reaches the set value. The inventors found that under this preferred embodiment, it is beneficial to combine the reaction process with the amount of each raw material, so that the prepared water-soluble hydrogel has a specific characteristic viscosity and shear viscosity, and the water-soluble polyester has the characteristics of rapid water solubility, good processing performance, and stable and uniform fiber opening.

[0056] In the present invention, the preparation method of the water-soluble polyester further comprises: extruding, pelletizing and drying the reactant II obtained by the polycondensation reaction, wherein the extrusion, pelletizing and drying methods can be carried out in conventional ways and equipment.

[0057] According to a particularly preferred embodiment of the present invention, the method for preparing the water-soluble polyester comprises the following steps:

[0058] (1) in the presence of tetrabutyl titanate, terephthalic acid and ethylene glycol are mixed in a weight ratio of 1.5-1.9:1, and reacted at a temperature of 230-260° C. and an absolute pressure of 0.2-0.4 MPa for 60-240 min to obtain a reactant I;

[0059] (2) After mixing the reactant I with sodium bis(hydroxyethyl)isophthalate-5-sulfonate (SIPE) and PEG2000, the mixture is first subjected to a temperature increase reaction at a temperature range of 260-275° C. for 40-50 min under an absolute pressure of 0.1-100 KPa, and then subjected to a final polycondensation reaction at a temperature of 270-285° C. and an absolute pressure of less than 100 Pa. After the stirring current reaches a set value, the cumulative polycondensation time is 70-85 min to obtain a reactant II, and the reactant II is extruded, pelletized, and dried to obtain a water-soluble polyester;

[0060] Wherein, relative to the total weight of terephthalic acid and ethylene glycol, the amount of tetrabutyl titanate is 0.0015-0.003wt%, the amount of SIPE is 4.5-7wt%, and the amount of PEG2000 is 4.5-7wt%; the amount ratio of SIPE to PEG2000 is 0.95-1.05:1.

[0061] The water-soluble polyester provided by the present invention is an environmentally friendly polyester that is quickly soluble in water. It has a specific characteristic viscosity and shear viscosity. When used in the spinning process, it can form a specific shear viscosity ratio with conventional polyester, effectively ensuring the uniformity of the distribution of the sea phase (the water-soluble polyester provided by the present invention) and the island phase (conventional polyester), thereby achieving the purpose of uniform distribution of the sea phase and the island phase in the fiber and fast and stable fiber opening speed. Based on this, the third aspect of the present invention provides the use of the above-mentioned water-soluble polyester and the water-soluble polyester prepared by the above-mentioned method in the production of chemical fibers. Among them, the chemical fiber can be a sea island fiber, etc.

[0062] The fourth aspect of the present invention provides a method for producing sea-island fibers, the method comprising the following steps: using the above-mentioned water-soluble polyester and / or the water-soluble polyester prepared according to the above-mentioned method as the sea phase and using conventional polyester as the island phase; wherein, at a temperature of 288°C and a shear rate of 6000s -1 Under the above conditions, the shear viscosity ratio of the water-soluble polyester to the conventional polyester is 0.8-0.9: 1. The sea-island fiber produced by the method is conducive to ensuring the formation of a stable sea-island phase distribution during the sea-island fiber forming process, and the fiber opening condition is good.

[0063] In the present invention, the spinning method can adopt a conventional spinning method or equipment. For example, the above-mentioned water-soluble polyester is dried as a sea phase, and the conventional polyester is dried as an island phase. The sea island yarn spinning device is used to spin the sea phase and the island phase to prepare the sea phase and the island phase of the fiber. The sea phase and the island phase are fed to the two screws A and B respectively to prepare the sea phase and the island phase of the fiber. The feeding speed of screw A is 12-18HZ, and the feeding speed of screw B is 32-28HZ, so that the weight ratio of the sea phase in the fiber is 25-35%, and the spinning speed is 2800-3200m / min.

[0064] When evaluating the spinning process of sea-island fibers, the cross-section of the raw silk was observed under a microscope, showing a clear morphology of uniformly distributed sea phase and island phase; the raw silk was stretched to prepare garter fabric, and the garter fabric was subjected to alkali reduction treatment in hot alkaline water to prepare ultrafine fibers. The weight loss rate of the garter after alkali reduction treatment was tested to be 31-33%, and the fiber opening condition of the garter was observed under an electron microscope to be good.

[0065] In the present invention, the conventional polyester can be a commercially available common polyester for preparing sea island fibers, or a polyester prepared by a conventional method in the art. Exemplarily, the preparation method of the conventional polyester comprises the following steps: ethylene glycol antimony catalyst, terephthalic acid (PTA) and ethylene glycol (EG) are mixed at a weight ratio of 1:2800-3200:1600-2000, and a conventional esterification reaction is carried out under the conditions of a gauge pressure of 0.2-0.3MPa and a temperature of 200-300°C; after the esterification reaction is completed, a pre-polycondensation reaction is carried out at 260-275°C for 40-50min, and finally the polycondensation reaction temperature is controlled at 270-285°C for a final polycondensation reaction, the absolute pressure is below 100Pa, and the cumulative polycondensation time is 100-110min after the stirring current of the reactor reaches the set value, and the melt is extruded by a melt pump, pelletized, and dried to obtain a conventional polyester.

[0066] The present invention will be described in detail below through examples.

[0067] In the following examples, unless otherwise specified, the raw materials and reagents used are conventional commercially available products.

[0068] In the following examples, the titanium content in the polyester was detected by elemental analysis; the content of sodium bis(hydroxyethyl)isophthalate-5-sulfonate unit (SIPE unit) and polyethylene glycol unit (PEG unit) was analyzed by hydrogen nuclear magnetic resonance spectroscopy. During the test, deuterated trifluoroacetic acid was used as the solvent and the polyester was analyzed by nuclear magnetic resonance spectroscopy. 1 According to H NMR test, the contents of SIPE units and PEG units were calculated based on the integrated areas of the corresponding characteristic peaks of the copolyester. The conversion rate of SIPE or PEG = (content calculated by NMR / theoretical addition amount) × 100%.

[0069] The intrinsic viscosity is tested and characterized according to 5.1 of GB / T14190-2017 Test Method for Fiber-Grade Polyester Chips.

[0070] The glass transition temperature (Tg), half crystallization period (t 1 / 2 ) was tested and calculated using differential scanning calorimetry (DSC). The specific process was as follows: under nitrogen protection, DSC thermal analysis was used to increase the temperature from 25°C to 290°C at a heating rate of 10°C / min, hold for 5 minutes, then cool down to 25°C at a rate of 400°C / min, then increase the temperature from 25°C to 290°C at a heating rate of 10°C / min, hold for 5 minutes, and finally cool down to 100°C at a rate of 10°C / min. The glass transition temperature Tg was calculated based on the second heating curve, and the crystallinity of the melt crystallization peak was used to calculate the half-crystallization period t in the melt crystallization process. 1 / 2 .

[0071] The shear viscosity is obtained by testing the rheological properties of samples using a capillary rheometer, wherein the capillary die diameter is 1 mm, the aspect ratio L / D=16, the inlet angle is 90°, the test temperature is 288°C, and the shear rate is 6000s -1 .

[0072] The alkali weight reduction treatment process is to treat the water-soluble polyester in an alkali solution with a temperature of 100° C. and an alkali content of 1 wt % for 45 minutes.

[0073] Example 1

[0074] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.191g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 471g of SIPE and 471g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 75min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6725g of a water-soluble polyester.

[0075] The water-soluble polyester obtained in Example 1 is 1 H NMR spectrum analysis showed that the chemical shifts of the sulfonate group of the characteristic unit SIPE unit were δ=8.97 and δd=9.06, and the chemical shifts of the PEG unit were δ=3.96 and δf=4.11.

[0076] Example 2

[0077] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.145g of tetrabutyl titanate catalyst were added, and a reaction I was carried out for 80min under the conditions of a gauge pressure of 0.3MPa and a temperature of 230°C to obtain a reactant I; after the reaction I was completed, 551g of SIPE and 551g of PEG 2000 were added to the reactant I in sequence, and the temperature was raised to react for 40min at a temperature range of 260-275°C under an absolute pressure of 0.1-100Kpa, and finally the polycondensation reaction temperature was controlled at 270°C and the absolute pressure was below 100Pa for a final polycondensation reaction. After the stirring current of the reactor reached the set value, the cumulative polycondensation time was 78min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6855g of a water-soluble polyester.

[0078] Example 3

[0079] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.187g of tetrabutyl titanate catalyst were added, and a reaction I was carried out for 240min under the conditions of a gauge pressure of 0.1MPa and a temperature of 260°C to obtain a reactant I; after the reaction I was completed, 394g of SIPE and 394g of PEG2000 were added to the reactant I in sequence, and the temperature was raised to react for 50min at a temperature range of 260-275°C under an absolute pressure of 0.1-100Kpa, and finally the polycondensation reaction temperature was controlled at 285°C and the absolute pressure was below 100Pa for a final polycondensation reaction. After the stirring current of the reactor reached the set value, the cumulative polycondensation time was 82min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6571g of a water-soluble polyester.

[0080] Example 4

[0081] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.141g of tetrabutyl titanate catalyst were added, and a reaction I of 150min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 432g of SIPE and 432g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 80min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6647g of a water-soluble polyester.

[0082] Example 5

[0083] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.235g of tetrabutyl titanate catalyst were added, and reaction I was carried out for 150min under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C; after the reaction I was completed, 401g of SIPE and 502g of PEG2000 were added in sequence, and the temperature was raised for 45min at a temperature range of 260-275°C under an absolute pressure of 0.1-100Kpa, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for the final polycondensation reaction. After the stirring current of the reactor reached the set value, the cumulative polycondensation time was 75min to obtain reactant II, and reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6686g of water-soluble polyester.

[0084] Example 6

[0085] The water-soluble polyester was prepared according to the method of Example 1, except that the amount of SIPE was replaced by 502 g, the amount of PEG2000 was replaced by 401 g, and the cumulative polycondensation time after the stirring current of the reactor reached the set value was replaced by 70 min; 6686 g of water-soluble polyester was obtained.

[0086] Example 7

[0087] The water-soluble polyester was prepared according to the method of Example 1, except that PEG2000 was replaced by PEG1500; 6725 g of water-soluble polyester was obtained.

[0088] Example 8

[0089] The water-soluble polyester was prepared according to the method of Example 1, except that tetrabutyl titanate was replaced by ethylene glycol titanium with an equimolar content of titanium element; 6725 g of water-soluble polyester was obtained.

[0090] Comparative Example 1

[0091] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.6624g of ethylene glycol antimony catalyst were added, and an esterification reaction was carried out for 200min at a gauge pressure of 0.25MPa and a temperature of 250°C. After the esterification reaction was completed, a temperature increase reaction was carried out at an absolute pressure of 0.1-100Kpa and a temperature range of 260-275°C for 45min. Finally, the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction. After the stirring current of the reactor reached the set value, the cumulative polycondensation time was 105min. The melt was extruded by a melt pump, pelletized, and dried to obtain 5783g of polyester (hereinafter referred to as conventional polyester).

[0092] Comparative Example 2

[0093] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.185g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 358g of SIPE and 358g of PEG2000 were added to the reactant I in sequence, and a temperature rise reaction was carried out at a temperature range of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 85min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6499g of polyester.

[0094] Comparative Example 3

[0095] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.200g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 635g of SIPE and 635g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 45min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 7053g of polyester.

[0096] Comparative Example 4

[0097] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.191g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 471g of SIPE and 471g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 64min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6725g of polyester.

[0098] Comparative Example 5

[0099] Polyester was prepared according to the method of Comparative Example 4, except that the cumulative polycondensation time after the stirring current of the reactor reached the set value was replaced with 91 minutes; 6725 g of polyester was obtained.

[0100] Comparative Example 6

[0101] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.120g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 471g of SIPE and 471g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 120min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6725g of polyester.

[0102] Comparative Example 7

[0103] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.285g of tetrabutyl titanate catalyst were added, and a reaction I of 200min was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 250°C to obtain a reactant I; after the reaction I was completed, 471g of SIPE and 471g of PEG2000 were added to the reactant I in sequence, and a temperature reaction was carried out at a temperature of 260-275°C under an absolute pressure of 0.1-100Kpa for 45min, and finally the polycondensation reaction temperature was controlled at 278°C and the absolute pressure was below 100Pa for a final polycondensation reaction, and after the stirring current of the reactor reached the set value, the cumulative polycondensation time was 46min to obtain a reactant II, and the reactant II (melt) was extruded through a melt pump, pelletized, and dried to obtain 6725g of polyester.

[0104] Test Example 1

[0105] The water-soluble polyesters or polyesters prepared in Examples 1 to 8 and Comparative Examples 1 to 7 were used as samples to calculate the heavy metal content (weight ratio wt%, heavy metal in Examples 1 to 8 and Comparative Examples 2 to 7 is titanium, and heavy metal in Comparative Example 1 is antimony), SIPE content (weight ratio wt%), and polyethylene glycol content (weight ratio wt%) in each sample, and the intrinsic viscosity of each sample was tested at a temperature of 288° C. and a shear rate of 6000 s -1 Shear viscosity under conditions, glass transition temperature Tg, half crystallization period t 1 / 2 And the water solubility under the alkali reduction process conditions, the results are shown in Table 1.

[0106] Table 1

[0107]

[0108] It can be seen from the data in Table 1 that the water-soluble polyesters obtained by the preparation method provided by the present invention in Examples 1 to 8 have a heavy metal content reduced by more than 95% compared with the conventional polyester provided in Comparative Example 1, and are highly environmentally friendly; the water solubility under the conditions of 100°C, 1.0% alkali content, and 45 minutes of alkali reduction process is more than 51.6%, which is more than 250 times higher than the water solubility of the conventional polyester obtained in Comparative Example 1, and has a significant characteristic of rapid water solubility; at the same time, the glass transition temperature and melt crystallization rate of the water-soluble polyesters obtained in Examples 1 to 8 are close to those of the conventional polyester obtained in Comparative Example 1, so the processing performance is better.

[0109] Test Example 2

[0110] The water-soluble polyester or polyester prepared in Examples 1 to 8 and Comparative Examples 2 to 7 was used as the sea phase, and the conventional polyester (polyester prepared in Comparative Example 1) was used as the island phase. After being dried respectively, the sea-island yarn was prepared using a sea-island yarn spinning device. The sea phase and the island phase were fed into screws A and B respectively to prepare the sea phase and the island phase of the fiber. The feeding speed of screw A was 15.00 Hz, and the feeding speed of screw B was 35.00 Hz. The weight ratio of the sea phase in the fiber was 30%. The spinning speed was 3000 m / min. The cross section of the yarn was observed using a microscope. When the water-soluble polyester prepared in Example 1 was used as the sea phase, the cross section of the sea-island phase of the sea-island yarn was as follows: Figure 1 As shown, it presents a clear morphology of uniform distribution of sea phase and island phase. When the polyester prepared in Comparative Example 2 is used as the sea phase, the cross section of the sea island phase of the sea island precursor is as follows: Figure 2 As shown in Figure 2, it shows that the marine phase and the island phase are adhered (see Figure 2 circled part).

[0111] The shear viscosity ratio of the water-soluble polyester or polyester obtained in Examples 1 to 8 and Comparative Examples 2 to 7 and the conventional polyester (polyester obtained in Comparative Example 1) was calculated. The results are shown in Table 2.

[0112] The sea-island raw yarn obtained above was drawn at a drawing speed of 450 m / min and a drawing ratio of 1.85. After the drawn yarn was woven into hosiery, the weight loss rate of the hosiery was tested under alkali weight reduction process conditions. The microscopic morphology (sea-island phase separation) of the hosiery after alkali weight reduction treatment was observed under an electron microscope. The results are shown in Table 2. Among them, when the water-soluble polyester prepared in Example 1 was used as the sea phase, the microscopic morphology of the hosiery after alkali weight reduction treatment was as follows: Figure 3 As shown, the fiber opening is uniform and complete, and the fiber opening condition is good. When the polyester prepared in Comparative Example 2 is used as the sea phase, the microscopic morphology of the garter after alkali reduction treatment is as follows Figure 4 As shown, the fiber opening condition is uneven.

[0113] Table 2

[0114] serial number Shear viscosity ratio Distribution of raw yarn cross section Garter water solubility % Garter opening condition Example 1 0.90 The marine and island phases are evenly distributed 32.5 good Example 2 0.80 The marine and island phases are evenly distributed 33.0 good Example 3 0.88 The marine and island phases are evenly distributed 31.8 good Example 4 0.84 The marine and island phases are evenly distributed 32.5 good Example 5 0.82 The marine and island phases are evenly distributed 32.8 good Example 6 0.89 The marine and island phases are evenly distributed 32.7 good Example 7 0.90 The marine and island phases are evenly distributed 32.7 good Example 8 0.90 The marine and island phases are evenly distributed 32.6 good Comparative Example 1 1.00 / / / Comparative Example 2 0.76 Marine and island phases are adhered 18.9 Uneven Comparative Example 3 1.08 Marine and island phases are adhered 38.5 Excessive reduction Comparative Example 4 0.73 Marine and island phases are adhered 28.4 Uneven, incomplete Comparative Example 5 1.16 Marine and island phases are adhered 19.8 Uneven, incomplete Comparative Example 6 0.60 Marine and island phases are adhered 24.9 Uneven, incomplete Comparative Example 7 1.14 Marine and island phases are adhered 31.2 Uneven, incomplete

[0115] From the data in Table 2, it can be seen that the sea phase and island phase interface of the sea-island yarn prepared by using the water-soluble polyester prepared in Examples 1 to 8 as the sea phase of the sea-island yarn is clear, and the garters prepared by the drawn yarn are evenly opened after alkali reduction. -1 The ratio of the shear viscosity under the conditions to the conventional polyester prepared in Comparative Example 1 is (0.8-0.9):1, which ensures the uniformity of the sea phase and island phase structure when applied to sea island yarns, so that the sea phase and island phase of the sea island yarns prepared using the water-soluble polyesters prepared in Examples 1 to 8 are evenly dispersed after being treated with an alkali reduction process.

[0116] In the process of forming sea-island yarns, two different melts, water-soluble polyester and conventional polyester, are compounded into fiber precursors with sea-island structures. Therefore, it is necessary to ensure that the two melts have appropriate shear viscosity to ensure that the sea phase and island phase structures are evenly distributed. When the shear viscosity difference between the two melts is too large, it will lead to uneven distribution of the sea phase and island phase structures and adhesion, and will also lead to uneven alkali reduction in the subsequent garter opening process. In addition, in order to ensure that the fiber has sufficient processing performance and use performance, it is necessary to ensure that its glass transition temperature Tg is not too low, otherwise the phenomenon of filament adhesion will occur during the processing, and its melt crystallization rate is slightly faster to ensure fiber strength. In the subsequent alkali reduction process of sea-island silk fabrics, users hope to reduce the heavy metal content in polyester as much as possible.

[0117] The polyester prepared in Comparative Example 1 has the properties of conventional polyester. The results show that the water solubility of the water-soluble polyesters prepared in Examples 1 to 8 is more than 250 times higher than that of conventional polyester.

[0118] The test results of Comparative Examples 2 and 3 show that when the SIPE and PEG contents are too high or too low, the water solubility and processing performance of the prepared polyester will be affected. When the content is too low, the water solubility rate of the polyester will decrease. When the content is too high, the polymerization reaction will be too fast and the shear viscosity of the polyester will be high, which will cause the cross-sectional distribution of the island silk to be uneven and excessive weight loss will occur.

[0119] The test results of Comparative Examples 4 and 5 show that too high or too low viscosity of the environmentally friendly polyester will break the balance of the melt pressure of the sea-island silk, resulting in uneven distribution of the sea phase and the island phase, and will also affect the stability of the alkali reduction of kelp silk.

[0120] Comparative Example 6 shows that when the catalyst content in the polyester synthesis system is too low, it will seriously affect the polymerization reaction rate and the processing performance of the obtained water-soluble polyester will deteriorate; Comparative Example 7 shows that when the catalyst content is too high, the polymerization reaction rate will be too fast, causing the copolymerization reaction to deteriorate in stability, and the obtained water-soluble polyester will have poor performance.

[0121] Taking into account the performance requirements of sea island silk, the preparation method of the water-soluble polyester provided in Examples 1 to 8 is adopted, and the amount of each raw material component, the reaction conditions and the content of specific components in the obtained water-soluble polyester are matched, so that the water-soluble polyester has the characteristics of low heavy metal content, rapid water solubility, good processing performance, stable and uniform fiber opening, and has significant functional and green effects.

[0122] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A water-soluble polyester, It is characterized in that The intrinsic viscosity of the water-soluble polyester is 0.50-0.55 dL / g, and the temperature is 288°C and the shear rate is 6000s -1 The shear viscosity under the conditions is 50-60Pa·s.

2. The water-soluble polyester according to claim 1, It is characterized in that The intrinsic viscosity of the water-soluble polyester is 0.515-0.53 dL / g, and the temperature is 288°C and the shear rate is 6000s -1 The shear viscosity under the conditions is 52-58.5 Pa·s; Preferably, the water-soluble polyester has a glass transition temperature of 55-68°C, a half-crystallization period of 2-4 minutes, and a water solubility of greater than or equal to 51.6% under alkali reduction process conditions of 100°C, 1 wt% alkali content, and 45 minutes.

3. The water-soluble polyester according to claim 1 or 2, It is characterized in that The water-soluble polyester contains sodium bis(hydroxyethyl)isophthalate-5-sulfonate units, polyethylene glycol units and titanium elements; Preferably, the polyethylene glycol unit is selected from at least one of PEG1500 unit, PEG2000 unit and PEG4000 unit; more preferably PEG2000 unit; Preferably, in the water-soluble polyester, the content of sodium bis(hydroxyethyl)isophthalate-5-sulfonate units is 6-8 wt %, the content of polyethylene glycol units is 6-8 wt %, and the content of titanium element is 0.0003-0.0005 wt %.

4. A method for preparing a water-soluble polyester, It is characterized in that The method comprises the following steps: (1) reacting a dibasic acid monomer with a diol monomer in the presence of a titanium catalyst to obtain a reactant I; (2) reacting the reactant I with sodium bis(hydroxyethyl)-5-sulfonate isophthalate and polyethylene glycol to react II; Among them, based on the total amount of the dibasic acid monomer and the diol monomer as 100 parts by weight, the amount of the titanium-based catalyst is 0.0015-0.003 parts by weight, the amount of sodium bis(hydroxyethyl)isophthalate-5-sulfonate is 4.5-7 parts by weight, and the amount of polyethylene glycol is 4.5-7 parts by weight.

5. The preparation method according to claim 4, It is characterized in that The dibasic acid monomer is selected from at least one of terephthalic acid, isophthalic acid and adipic acid; preferably terephthalic acid; The diol monomer is ethylene glycol and / or pentanediol; preferably ethylene glycol; The polyethylene glycol is selected from at least one of PEG1500, PEG2000 and PEG4000; preferably PEG2000; The titanium-based catalyst is tetrabutyl titanate and / or titanium glycol; preferably tetrabutyl titanate.

6. The preparation method according to claim 4 or 5, It is characterized in that The weight ratio of the dibasic acid monomer to the diol monomer is 1-2.5:1; more preferably 1.5-1.9:1; Preferably, the usage ratio of the sodium bis(hydroxyethyl)isophthalate-5-sulfonate to the polyethylene glycol is 0.79-1.26:1, more preferably 0.95-1.05:

1.

7. The preparation method according to claim 4 or 5, It is characterized in that The conditions of reaction I in step (1) include at least: temperature of 230-260° C., absolute pressure of 0.2-0.4 MPa, and time of 60-240 min.

8. The preparation method according to claim 4 or 5, It is characterized in that The process of reaction II in step (2) includes: firstly performing a pre-polycondensation reaction and then performing a final polycondensation reaction; Preferably, the conditions of the pre-polycondensation reaction at least include: a temperature rise reaction in the range of 260-275°C, an absolute pressure of 0.1-100 KPa, and a time of 40-50 min; The conditions of the final polycondensation reaction include at least: a temperature of 270-285° C., an absolute pressure of less than 100 Pa, and a time of 70-85 min.

9. Use of the water-soluble polyester according to any one of claims 1 to 3 or the water-soluble polyester prepared according to the method according to any one of claims 4 to 8 in the production of chemical fibers.

10. A method for producing sea-island fibers, It is characterized in that The method comprises the following steps: using the water-soluble polyester described in any one of claims 1 to 3 and / or the water-soluble polyester prepared according to the method described in any one of claims 4 to 8 as the sea phase and using conventional polyester as the island phase; wherein, at a temperature of 288°C and a shear rate of 6000s -1 Under the conditions, the shear viscosity ratio of the water-soluble polyester to the conventional polyester is 0.8-0.9:1.

Citation Information

Patent Citations

  • Method for preparing water-soluble polyester based on aluminum compound as catalyst

    CN102558527A

  • Easily hydrolytic degradation polyester, and synthetic method thereof

    CN108003332A

  • Industrial continuous manufacturing method of normal-pressure easy cation-dyeable polyester chip

    CN113004505A

  • Modified poly ester and its preparing method

    CN1587297A

  • Alkali soluble polyester and its preparation method

    CN1869097A