Gel composite material, water photovoltaic power generation device and preparation method and application of water photovoltaic power generation device
By using a combination of hydrophobic insulated porous materials and ionic temperature-sensitive hydrogels in hydrovoltaic power generation devices, combined with photothermal function fillers, the problem of low heat transfer efficiency of traditional hydrovoltaic power generation devices is solved, and efficient seawater evaporation and electricity are achieved Output has expanded its application in seawater desalination and new energy fields.
Patent Information
- Application Number
- CN202411263579.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-10
AI Technical Summary
Due to the two-dimensional structure, traditional hydrovoltaic power generation devices have low heat transfer efficiency and large heat loss, so they cannot achieve high evaporation efficiency, high power collection and universal applications at the same time, which limits their application in the field of efficient seawater desalination in multiple scenarios.
Hydrophobic insulated porous materials are used as the framework to fill ionic temperature-sensitive hydrogels, combined with photothermal fillers, to form gel composite materials with respiration effects, and to achieve seawater evaporation and synchronous output of electrical energy using temperature gradient and wettability differences.
It realizes efficient seawater evaporation and desalination, and outputs high-power DC power, which improves the application potential of seawater desalination and new energy development, and has material universality and structural simplicity.
Smart Images

Figure CN118895015A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional gel materials, and specifically relates to a gel composite material, a water-voltaic power generation device, its preparation method and application. Background Technology
[0002] Hydrovoltaic power generation devices (HPV devices) are characterized by miniaturization, low cost, high evaporation efficiency, and high adaptability. They can realize functions such as energy harvesting, clean water collection, and self-powered equipment applications in seawater environments and other wastewater scenarios, making them one of the important directions for the development of seawater desalination. Developing high-efficiency HPV devices to achieve efficient seawater desalination is of great significance to the sustainable development of the global water environment. The development and application of novel HPV devices are conducive to promoting the active harvesting of environmental energy and the utilization and collection of solar energy, which is of great significance to the development, utilization, recycling, and sustainable environmental development of new energy sources. However, traditional HPV devices are mostly two-dimensional structures with low heat transfer efficiency and large heat loss. They can usually only output electricity under sunlight conditions, and in particular, they cannot simultaneously achieve high evaporation efficiency, high energy collection, and universal application, which greatly limits their application in the field of efficient seawater desalination in various scenarios. Researching HPV devices that can simultaneously output electricity, autonomously absorb solar energy and convert it into heat energy, realize solar interface evaporation, and achieve high-power HPV power generation in multiple scenarios is of great significance for the efficient utilization of seawater desalination, alleviating the crisis of traditional mineral energy, and expanding the field of new energy sources. Summary of the Invention
[0003] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to provide a gel composite material, a water-voltaic power generation device, a preparation method thereof, and its application.
[0004] This invention provides a gel composite material, characterized in that the gel composite material uses a hydrophobic insulating porous material as a skeleton, and the skeleton is filled with an ion-temperature-sensitive hydrogel; wherein the ion-temperature-sensitive hydrogel is a hydrogel modified with anionic or cationic groups; wherein the hydrogel modified with anionic or cationic groups is a cross-linked hydrogel of a cationic modifier or anionic modifier and a matrix material, and the mass ratio of the matrix material to the ion modifier in the ion-temperature-sensitive hydrogel is 10:1 to 1:1;
[0005] The matrix material includes one or more of poly(N-isopropylacrylamide) PNIPAM, poly(N-vinylcaprolactam) PNVCL, poly(sebacic anhydride) PSPA, and poly(N-acryloylglycamide) PNAGA; the anionic modifier includes at least one of 2-acrylamido-2-methylpropanesulfonic acid AMPS and dimethylaminoethyl methacrylate DMAEMA; and the cationic modifier includes at least one of (3-acrylamidopropyl)trimethylammonium chloride MPTAmC and dimethylaminopropylacrylamide DMAPAA.
[0006] The hydrophobic insulating material has hydrophobic or water-repellent properties.
[0007] The ion-temperature-sensitive hydrogel is a hydrogel with different wettability at different temperatures.
[0008] The ion-thermosensitive hydrogel has different hydrophobic or hydrophilic properties under different temperature conditions. Under light conditions, the upper and lower surfaces exhibit different wettability, and water is continuously pumped from the bottom to the upper surface, exhibiting a respiration effect similar to that of plant branches.
[0009] In the preparation of thermosensitive hydrogels, an appropriate proportion of anion / cation modifier monomers are introduced to form ion-modified thermosensitive hydrogels, thereby improving the ion selectivity within the hydrogel. During seawater evaporation, the ionic groups enhance electrostatic water capture capacity, promote efficient water transport, and improve seawater desalination efficiency. Simultaneously, the ionic groups can promote the separation of anions and cations in the water, improving the power generation efficiency of hydrovoltaic devices.
[0010] Preferably, the hydrophobic insulating porous material has vertically penetrating internal channels.
[0011] Preferably, the hydrophobic insulating porous material is a hydrophobic insulating porous material with photothermal conversion function.
[0012] Preferably, the hydrophobic insulating porous material with photothermal conversion function includes: a hydrophobic insulating porous material containing photothermal functional filler or an intrinsically black hydrophobic insulating porous material without photothermal functional filler.
[0013] Furthermore, the mass percentage of the photothermal functional filler in the hydrophobic insulating porous material containing the photothermal functional filler is 1wt%~10wt%.
[0014] Preferably, the photothermal functional filler includes one or more of the following: carbon powder, carbon black, carbon nanotubes, graphene, graphite, amorphous carbon, MXene, metal-organic frameworks (MOFs), and azobenzene. The functional filler converts light energy into heat energy, providing thermal energy for seawater evaporation.
[0015] Preferably, the hydrophobic insulating porous material containing photothermal functional filler includes one or more of aerogel, foam plastic, and porous wood containing photothermal functional filler.
[0016] The aerogel is one or more of unmodified aerogel and hydrophobic and / or insulating modified aerogel; the foam plastic is one or more of unmodified foam plastic and hydrophobic and / or insulating modified foam plastic; the porous wood is one or more of unmodified porous wood and hydrophobic and / or insulating modified porous wood.
[0017] Further, the aerogel is at least one of inorganic aerogel, organic aerogel, and organic / inorganic aerogel composite material; wherein the inorganic aerogel includes one or more of TiO2 aerogel, SiO2 aerogel, and SiC fiber aerogel; the organic aerogel includes one or more of TEMPO oxidized cellulose aerogel (TCNF), microcrystalline cellulose aerogel, polyvinylidene fluoride aerogel, polyacrylonitrile aerogel, and poly(vinylidene fluoride-co-hexafluoropropylene) aerogel; and the organic / inorganic aerogel composite material includes one or more of TCNF / MXene aerogel, ethyl cellulose / Fe3O4 aerogel, and TCNF / TiO2 aerogel.
[0018] Preferably, the foamed plastic is one or more of polystyrene foam, polypropylene foam, polyethylene foam, polycarbonate foam, polytetrafluoroethylene foam, polyvinyl chloride foam, polyamide foam, polyurethane foam, polyester foam, phenolic resin foam, epoxy resin foam, and polyvinyl alcohol foam; the porous wood is one or more of intrinsically hydrophobic modified wood, physically modified porous wood, and chemically modified porous wood; wherein the wood includes one or more of poplar, willow, paulownia, sycamore, birch, red pine, and grass.
[0019] Preferably, the intrinsic black hydrophobic insulating porous material without photothermal functional fillers includes one or more of foam plastics and porous wood without photothermal functional fillers; wherein the foam plastic is one or more of unmodified foam plastics and foam plastics modified with hydrophobicity and / or insulation; and the porous wood is one or more of unmodified porous wood and porous wood modified with hydrophobicity and / or insulation.
[0020] Preferably, the foamed plastic is one or more of polystyrene foam, polypropylene foam, polyethylene foam, polycarbonate foam, polytetrafluoroethylene foam, polyvinyl chloride foam, polyamide foam, polyurethane foam, polyester foam, phenolic resin foam, epoxy resin foam, and polyvinyl alcohol foam. Preferably, the porous wood is one or more of intrinsically hydrophobic modified wood, physically modified porous wood, and chemically modified porous wood; wherein the wood includes one or more of poplar, willow, paulownia, sycamore, birch, red pine, and other woods.
[0021] Preferably, the hydrophobic modification is one or more of surface micro / nano structure construction and surface hydrophobic coating processing; wherein the surface micro / nano structure construction method includes one or more of etching, engraving, sol-gel method, and laser printing; the surface hydrophobic coating processing includes one or more of surface coating and immersion treatment; the materials used in the surface hydrophobic coating processing include one or more of fluorine-containing coatings (e.g., 1H, 1H, 2H, 2H-perfluorooctyltrichlorosilane, perfluorodecyltriethoxysilane), silicon-containing coatings (e.g., methyltrimethoxysilane, hexadecyltrimethoxysilane, vinyltrimethoxysilane), and aliphatic chain-containing coatings (e.g., polylactic acid, hexadecyltrimethoxysilane).
[0022] Preferably, the insulation modification is one or more of surface insulation treatment and impregnation insulation treatment; the material used for the insulation modification is at least one of organic insulating material, inorganic insulating material, and organic / inorganic composite insulating material.
[0023] Preferably, the organic insulating material is one or more of organosilicon resin, phenolic resin, epoxy resin, and polyimide; the inorganic insulating material is one or more of phosphate, silicate, TiO2, Cr2O3, MgO, ZrO2, SiO2, and Al2O3; and the composite insulating material is one or more of SrTiO3 modified resin, SiO2 / SiC modified resin, Fe3O4 / SiO2 modified resin, and SiO2 modified resin.
[0024] More preferably, the aerogel is polyvinylidene fluoride (PVDF) aerogel. PVDF is a chemically stable material that can withstand various corrosive environments, including acids and alkalis. It has broad application potential in seawater desalination. Aerogels, as materials with a three-dimensional porous structure, low density, and excellent mechanical properties, are widely used in water purification. PVDF aerogels maintain their original porous structure even at high temperatures; the aerogel material exhibits minimal shrinkage, high strength, and stable porosity and specific surface area. Due to its porous structure, the aerogel has a very high water absorption rate, and even under strong acid and alkali environments, its service life is minimally affected. PVDF itself is electronegative; during seawater desalination, it can promote the separation of anions and cations in the water, generating a potential energy difference that enables hydroelectric power generation.
[0025] The aerogel is prepared by one or more of the following methods: sol-gel method, inorganic aluminum salt method, rapid gelation method, template method, emulsion method, impregnation method, chemical vapor deposition method, three-dimensional printing method, phase exchange method, and carbothermal reduction reaction method, and is obtained by drying. The drying method is supercritical drying, subcritical drying, freeze drying, vacuum drying, atmospheric pressure drying, conduction drying, and distillation drying.
[0026] Preferably, the aerogel preparation method is a phase exchange method. The solvent used for the aerogel is dimethyl sulfoxide (DMSO), and the proportion of polyvinylidene fluoride (PVDF) is 3wt%~30wt%. PVDF is soluble in DMSO. Since the freezing point of DMSO is 18.25℃, and water is a non-solute in the PVDF solution, the PVDF solution can undergo phase exchange in an aqueous environment at 0℃~18.25℃, exchanging the solidified DMSO for water, followed by drying.
[0027] The drying method is supercritical drying or freeze drying.
[0028] More preferably, the aerogel is prepared using a unidirectional freeze-drying method. The solvent is poured into a bottom metal mold and placed in a liquid nitrogen environment for freezing. The solution crystallizes first at the bottom, and the ice crystals grow upwards through a vertical temperature gradient, forming vertically penetrating pores. This improves the long-term salt resistance of the hydrovoltaic power generation device, meeting the requirements for long-term application. Preparation of the gel composite material: A hydrogel solution is pumped into the material using a vacuum pump, and the hydrogel solution reacts inside the aerogel to form a hydrogel.
[0029] For example, polyvinylidene fluoride aerogel containing photothermal functional fillers is obtained by directional freezing of a DMSO solution containing polyvinylidene fluoride and raw materials for photothermal functional fillers.
[0030] This invention provides a method for preparing a gel composite material, comprising:
[0031] (1) Mix the matrix monomer, crosslinking agent, initiator, modifier and solvent to obtain a mixed solution;
[0032] (2) The hydrophobic insulating porous material is immersed in a mixed solution, vacuum filtered, cooled, and then immersed in a catalyst solution under protective gas conditions for crosslinking to obtain a gel composite material.
[0033] Preferably, in step (1), the matrix monomer is one or more of N-isopropylacrylamide (NIPAM), N-vinylcaprolactam (NVCL), sebacic anhydride (SPA), and N-acryloylglycamide (NAGA); the crosslinking agent is N,N-methylenebisacrylamide (MBAA); the initiator is ammonium persulfate (APS); and the solvent is deionized water.
[0034] In step (1), the monomer in the mixed solution accounts for 3 wt% to 10 wt% of the solvent mass, the crosslinking agent accounts for 0.01 wt% to 0.1 wt% of the solvent mass, the initiator accounts for 0.1 wt% to 1 wt% of the solvent mass, and the modifier accounts for 0.3 wt% to 10 wt% of the solvent mass.
[0035] The crosslinking time in step (2) is 5-12 hours.
[0036] Preferably, in step (2), the temperature is cooled to 2-8°C; the protective gas is nitrogen; the catalyst is tetramethylethylenediamine (TEDMA); and the concentration of the catalyst solution is 0.5wt%~1wt%.
[0037] The present invention provides a water-based photovoltaic power generation device, which includes any of the described gel composite materials or a gel composite material prepared by any of the described gel composite materials preparation methods, and electrodes.
[0038] The electrode includes a positive electrode and a negative electrode; electrodes are respectively provided on the top and bottom of the gel composite material; wherein the positive electrode and the negative electrode are arranged in parallel.
[0039] The electrode material is a porous electrode; wherein the porous electrode is a metal foam electrode or a graphite felt electrode; wherein the metal foam electrode includes one or more of foamed copper electrodes, foamed stainless steel electrodes, foamed iron-nickel electrodes, foamed nickel electrodes, foamed titanium electrodes, and foamed aluminum electrodes;
[0040] More preferably, the metal foam electrode is a strip-shaped copper foam electrode, which is embedded at different positions in the vertical direction of the material to collect the water voltaic energy generated by the separation of positive and negative ions in the solution.
[0041] Preferably, the electrode spacing is 0.5 cm to 10 cm, and it is built into the upper and lower parts of the gel composite material to collect the electrical energy generated by seawater ion separation.
[0042] More preferably, the foam metal electrode is a strip-shaped foam copper electrode, with the upper and lower electrodes spaced 1cm-10cm apart.
[0043] The electrode is connected to an external energy harvesting device via a wire.
[0044] The water-based photovoltaic power generation device continuously outputs electrical energy during the evaporation of water to power electrical appliances.
[0045] The water-based photovoltaic power generation device is designed and molded based on gel composite materials, and achieves different power outputs under different solutions and environmental conditions.
[0046] The hydroelectric power generation device continuously outputs electrical energy during the seawater evaporation process to power electrical appliances.
[0047] The water evaporation function refers to one or more types of water, including ultrapure water, distilled water, deionized water, tap water, river water, lake water, seawater, rainwater, industrial wastewater, domestic sewage, and agricultural wastewater; the water-based photovoltaic power generation is electrostatic energy generated through the separation of positive and negative ions in the solution.
[0048] The aforementioned hydroelectric power generation device can achieve seawater evaporation and desalination, while simultaneously generating hydroelectric power output.
[0049] The present invention provides a method for preparing a hydrovoltaic power generation device, which includes: assembling electrodes on a gel composite material, or assembling electrodes in situ during the preparation of the gel composite material.
[0050] Specifically, the process includes: mixing matrix monomers, crosslinking agents, initiators, modifiers, and solvents to obtain a mixed solution; immersing a hydrophobic insulating porous material in the mixed solution, vacuum filtering, cooling, and then immersing it in a catalyst solution for crosslinking for 5-12 hours under protective gas conditions to obtain a gel composite material; assembling electrodes to obtain a hydrovoltaic power generation device.
[0051] Alternatively, the matrix monomer, crosslinking agent, initiator, modifier, and solvent can be mixed to obtain a mixed solution; the hydrophobic insulating porous material equipped with electrodes can be immersed in the mixed solution, vacuum filtered, cooled, and then immersed in a catalyst solution for crosslinking for 5-12 hours under protective gas conditions to obtain a water-voltaic power generation device.
[0052] This invention provides an application of the aforementioned water-based photovoltaic power generation device or a water-based photovoltaic power generation device prepared by the aforementioned method in the fields of environment, new energy, and renewable resources.
[0053] Preferably, the applications in the environmental field include one or more of the following: seawater desalination, wastewater treatment, distilled water collection, and biomimetic plant materials.
[0054] The new energy field includes one or more of solar power generation and hydroelectric power generation;
[0055] The renewable resources sector includes one or more of the following: plant growth monitoring, ecosystem services, ecosystem restoration, and water energy harvesting.
[0056] This invention develops a water-based photovoltaic (VPC) power generation device with a breathing effect, which can simultaneously meet the requirements of high-power generation, high evaporation efficiency, and long-term practicality, and is expected to achieve efficient utilization of solar energy and seawater resources. This VPC power generation device possesses an intrinsic photothermal evaporation effect, which can convert solar energy into thermal energy. It also has enhanced VPC power generation capabilities through ionic group enhancement, enabling autonomous power generation and output of electrical energy through the separation of positive and negative charges in water, simultaneously achieving seawater evaporation and efficient desalination. This VPC power generation device features universally applicable materials, simple structure, easy processing and development, and multi-scenario applications, showing great promise in the field of new energy.
[0057] This invention relates to a hydrovoltaic device and its application powered by an ion-temperature-sensitive hydrogel. The device comprises a hydrophobic, insulating porous material (photothermal functional filler), an ion-temperature-sensitive hydrogel with a breathing effect filled within the pores, and electrodes. Specifically, the porous material has photothermal conversion capabilities, creating a temperature gradient across the material to drive water evaporation. The temperature-sensitive hydrogel filled within the porous material can directionally regulate the wettability of the pores. Under illumination, the temperature-sensitive hydrogel near the upper surface contracts upon heating, decreasing its hydrophilicity and promoting a gradient wettability across the porous material, achieving a self-transport effect similar to the vascular bundles of a tree trunk, thus facilitating water evaporation and outflow. Ion modification imparts ion selectivity to the porous material and enhances its water absorption and capture capabilities. Compared to ion-doped hydrogels, ion-modified hydrogels exhibit greater stability and can generate electricity autonomously under both light and dark conditions, maintaining stable output for extended periods, significantly improving seawater evaporation efficiency and all-weather power output efficiency. This invention is the first to realize a hydrophobic insulating porous material empowered by ion-temperature-sensitive hydrogel, enabling seawater evaporation, desalination and simultaneous power generation. That is, in the process of seawater desalination, the chemical energy of ions in the solution is converted into electrical energy, and its electrical output can be stored or used to power electrical appliances, which greatly expands the application in the fields of seawater desalination and new energy development.
[0058] Beneficial effects
[0059] Compared to existing technologies, this invention employs a combination of hydrophobic insulating porous materials and functional temperature-sensitive hydrogels, enabling simultaneous seawater desalination and hydro-voltaic power generation. For example, the photothermal filler within the porous material utilizes the physical photothermal transfer effect to achieve rapid heat accumulation on the material's surface, creating a thermal gradient that drives water evaporation. The temperature-sensitive hydrogel embedded within the porous material utilizes its wettability differences at different temperatures to achieve gradient wettability on the material's upper and lower surfaces, further allowing for directional control of pore size changes, achieving a function similar to water transport in tree trunk vessels. The introduction of ionic segments into the temperature-sensitive hydrogel imparts ion selectivity, enabling use in multiple scenarios and improving the device's power output and long-term performance stability. Compared to other hydro-voltaic power generation devices, this invention utilizes a low-cost, simple formulation and assembly technology to achieve high evaporation / desalination efficiency and high-power DC output for hydro-voltaic power generation.
[0060] Based on the research results of this invention, the developed hydroelectric power generation device can achieve a seawater evaporation rate of up to 2.75 kg / (m²). 2 *h). Based on this effect, the present invention also provides the aforementioned hydrovoltaic power generation device for obtaining DC power during seawater evaporation / desalination.
[0061] This invention discloses a hydro-voltaic power generation device, its preparation method, and its applications. The evaporator is based on a hydrophobic, insulating, photothermal porous material and ion-temperature-sensitive hydrogel with controlled wettability. It possesses efficient photothermal conversion effects and positive and negative ion separation capabilities, creating a temperature and wettability gradient across the material to promote water evaporation and ion separation. This simultaneously achieves seawater desalination and hydro-voltaic power generation, while also collecting electrical energy and desalinated water. This invention is the first to integrate ion-temperature-sensitive hydrogel into a hydrophobic, photothermal porous material, enabling simultaneous high-efficiency seawater desalination, hydro-voltaic power collection, and plant irrigation, greatly expanding the application of hydro-voltaic power generation devices in agriculture and new energy fields.
[0062] The high-efficiency hydro-voltaic power generation device provided by this invention is simple to manufacture, low in cost, and widely applicable. It has low requirements for materials, equipment, and environment, and exhibits high photothermal conversion efficiency, strong hydro-voltaic power generation, and great potential for large-scale production. Typically, the hydro-voltaic power generation device can output 23.33 uw / cm² in seawater desalination. 2 The collected freshwater can be used for agricultural irrigation, and the collected electricity can drive low-power electronic devices. This has important implications and promotes the improvement of seawater evaporation efficiency and hydroelectric power generation efficiency, as well as the construction and development of self-irrigation ecosystems. Attached Figure Description
[0063] Figure 1 This is a physical image of the PAN-PNIPAM-DMAEMA hydrovoltaic power generation device described in Example 1;
[0064] Figure 2 This is a cross-sectional scanning electron microscope image of the PAN-PNIPAM-DMAEMA hydrovoltaic device described in Example 1;
[0065] Figure 3 These are physical images and thermal images of the PNIPAM hydrogel as a function of temperature in Example 1;
[0066] Figure 4 This is a graph showing the change in water evaporation mass over time under 1.0 sun light intensity irradiation of the PVDF-PNIPAM-AMPS hydrovoltaic power generation device described in Example 2.
[0067] Figure 5 This is a graph showing the change of interface evaporation temperature over time for the PVDF-PNIPAM-AMPS hydrovoltaic power generation device described in Example 2 under 1.0 sun light intensity irradiation;
[0068] Figure 6 The current-voltage curve of the PVDF-PNIPAM-AMPS hydrovoltaic power generation device described in Example 2, measured by an electrochemical workstation;
[0069] Figure 7The photovoltaic power output of a single PNVCL-AMPS-wood photovoltaic power generation device as described in Example 3;
[0070] Figure 8 The photovoltaic power output of a single PNAGA-DMAEMA-EVA foam photovoltaic power generation device as described in Example 4;
[0071] Figure 9 The hydrovoltaic power output of a single TCNF-DMAPAA-PSPA aerogel hydrovoltaic power generation device as described in Example 5;
[0072] Figure 10 The hydrovoltaic power output of a single PVDF-PNIPAM-MPTAmC aerogel hydrovoltaic power generation device as described in Example 6;
[0073] Figure 11 The output of the single (PVDF-HFP)-NIPAM-AMPS voltaic generator described in Example 7 under different simulated water samples;
[0074] Figure 12 These are actual images and ultraviolet spectra of the water quality before and after desalination using the microcrystalline-PNIPAM-AMPS hydrovoltaic power generation device described in Example 8. Detailed Implementation
[0075] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0076] The raw materials used in the examples are as follows:
[0077] Polyacrylonitrile: from Shanghai Titan Technology Co., Ltd., model: RG, weight average molecular weight: 50,000, item number: 013358765;
[0078] Dimethyl sulfoxide: from Shanghai Titan Technology Co., Ltd., model and specifications: AR, ≥99.0% (GC), part number: 01104495;
[0079] N-Isopropylacrylamide: From Shanghai Aladdin Biochemical Technology Co., Ltd., Model and Specification: 98%, Product No.: I106818-100g;
[0080] Carbon nanotubes: from Shanghai Aladdin Biochemical Technology Co., Ltd., specifications: >95%, outer diameter: 8-15nm, length: ~50μm, specific surface area >140m². 2 / g, Product No.: C313046-5g;
[0081] Hexadecyltrimethoxysilane: from Shanghai Titan Technology Co., Ltd., model and specifications: RG, 98%+, part number: 01030566;
[0082] N,N-Methylenebisacrylamide: from Shanghai Aladdin Biochemical Technology Co., Ltd., model and specification: CP, 97%, item number: M104022-25g;
[0083] Foam metal electrode: from Jinyihe New Materials Business Department, Chengnan, Wuzhong Economic Development Zone; Model and specifications: 1.8*200*300mm.
[0084] Dimethylaminoethyl methacrylate: from Ron Reagents, model and specification: 99.9% (GC), catalog number: R096935-500ml;
[0085] Tetramethylethylenediamine: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 99%, item number: N818999-1L;
[0086] Polyvinylidene fluoride: from Shanghai Yuanye Biotechnology Co., Ltd., model and specifications: 5um, 99.9%, molecular weight 600,000, item number: S27372-500g;
[0087] 2-Acrylamide-2-methylpropanesulfonic acid: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 98%, item number: A800508-100g;
[0088] Sodium chloride: from Sinopharm Chemical Reagent Co., Ltd., model: AR (Shanghai Test), ≥99.5%, item number: 10019318
[0089] Amorphous carbon: from Shanghai McLean Biochemical Technology Co., Ltd., model and specifications: 400 mesh, powder, item number: C829813-100g;
[0090] dodecanethiol: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 98%, item number: D806874-25ml;
[0091] N-Vinylcaprolactam: From Shanghai Maclean Biochemical Technology Co., Ltd., Model and Specification: 99%, Product No.: N838648-2g;
[0092] Vinyltrimethoxysilane: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 98%, item number: V823925-25ml;
[0093] Ammonium persulfate: from Sinopharm Chemical Reagent Co., Ltd., model and specification: AR (Shanghai Test), ≥98.0%, item number: 10002616;
[0094] N-Acryloylglycine: From Shanghai Yuanye Biotechnology Co., Ltd., Model and Specification: 98%, Product No.: Y69205-250mg;
[0095] TEMPO oxidized cellulose: from Beijing Shansheng Technology Co., Ltd.;
[0096] Polydimethylsiloxane: from Shanghai Maclean Biochemical Technology Co., Ltd., item number: D849784;
[0097] 1H, 1H, 2H, 2H-Perfluorooctyltrichlorosilane: from Sinopharm Chemical Reagent Co., Ltd., model and specification: 97%, item number: XW785604591;
[0098] Graphene: from Saen Chemical Technology (Shanghai) Co., Ltd., model and specifications: particle size: 7-12μm, number of layers: 1-3, 98%, item number: A62053;
[0099] Sebacic anhydride: from Saen Chemical Technology (Shanghai) Co., Ltd., model and specification: 98%, item number: A010415;
[0100] Dimethylaminopropylacrylamide: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 98%, item number: N838796-5g;
[0101] (3-Acrylamidopropyl)trimethylammonium chloride: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 74-76%, item number: A838630-5ml;
[0102] Poly(vinylidene fluoride-co-hexafluoropropylene): From Shanghai Maclean Biochemical Technology Co., Ltd., Model and Specifications: Weight Average Molecular Weight: 400,000, Number Average Molecular Weight: 130,000, Item No.: P875306-1g;
[0103] Microcrystalline cellulose: from Shanghai Maclean Biochemical Technology Co., Ltd., model and specification: 100-200 mesh, item number: M909921-100g;
[0104] Graphite powder: from Shanghai Aladdin Biochemical Technology Co., Ltd., model and specifications: 99.95%, ≥325 mesh, item number: G123645-100g.
[0105] Example 1
[0106] In this embodiment, a water-based photovoltaic power generation device is provided, and its preparation method is as follows:
[0107] A 6wt% solution of polyacrylonitrile (PAN) was prepared by dissolving polyacrylonitrile (PAN) in dimethyl sulfoxide (DMSO). 5wt% carbon nanotubes were added to the solution, and the mixture was stirred until homogeneous to obtain an aerogel solution. 4cm × 2cm foamed iron-nickel electrodes with a 2cm gap were placed in a unidirectionally frozen mold. The sol was poured into the mold, and the mixture was then frozen in liquid nitrogen for 1 h, exchanged under deionization conditions at 2–8℃ for 48 h, and then freeze-dried for 48 h to obtain a PAN aerogel. The PAN aerogel was then subjected to chemical vapor deposition (CVD) with hexadecyltrimethoxysilane (90℃, 5 h) to obtain a hydrophobically modified PAN aerogel. Two parallel foamed iron-nickel electrodes, spaced 2cm apart, were embedded in the aerogel, with the lower electrode and bottom separated by a 2cm gap.
[0108] A NIPAM-DMAEMA solution was prepared by dissolving 5 wt% N-isopropylacrylamide (NIPAM), 0.1 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 0.5 wt% dimethylaminoethyl methacrylate (DMAEMA) in deionized water. An aerogel was then immersed in this solution, and the solution was subjected to vacuum filtration. The aerogel filled with the hydrogel solution was cooled to 2-8°C. Under nitrogen atmosphere, the aerogel was then immersed in a 0.6 wt% tetramethylethylenediamine solution for 12 hours to crosslink, allowing the hydrogel inside the PAN aerogel to crosslink in situ. This yielded a PAN-PNIPAM-DMAEMA aerogel (named PAN-PD). A foamed iron-nickel electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0109] like Figure 1 The image shown is a physical diagram of this hydroelectric power generation device. Figure 2 The image shows a cross-sectional scanning electron microscope image of a hydrovoltaic device. As can be seen from the image, region 1 is a vertically penetrating aerogel channel, and region 2 is the dried hydrogel attached to the aerogel channel. Figure 3 These are physical images and thermal images of the PNIPAM hydrogel as it changes with temperature. The hydrogel undergoes a phase transition as it heats from 33 degrees to 41.4 degrees.
[0110] Example 2
[0111] In this embodiment, a hydrovoltaic power generation device is provided, which is prepared as follows: Polyvinylidene fluoride (PVDF) is dissolved in dimethyl sulfoxide to prepare an 8wt% solution. 4wt% graphite powder is added to the solution, and the mixture is stirred until homogeneous to obtain an aerogel solution. 4cm × 2cm foamed iron-nickel electrodes with a 3cm gap are placed in a unidirectionally frozen mold. The above sol is poured into the mold, and then the mixture is frozen in liquid nitrogen for 2 hours, exchanged in a deionization environment at 2-8℃ for 48 hours, and then freeze-dried for 48 hours to obtain polyvinylidene fluoride (PVDF) aerogel. The two parallel foamed iron-nickel electrodes are spaced 3cm apart and embedded in the aerogel, with the lower electrode and the bottom separated by 2cm.
[0112] A NIPAM solution was prepared by dissolving 10 wt% N-isopropylacrylamide (NIPAM), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 6 wt% 2-acrylamide-2-methylpropanesulfonic acid (AMPS) in deionized water. An aerogel was then immersed in the NIPAM solution, and the solution was subjected to vacuum filtration. The aerogel filled with the hydrogel solution was cooled to 2-8 degrees Celsius. Under nitrogen atmosphere, the aerogel was then immersed in a 0.5% tetramethylethylenediamine solution for 12 hours to crosslink the hydrogel internally, resulting in a PVDF-PNIPAM-AMPS aerogel (named PPA). A foamed iron-nickel electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0113] Figure 4 This is a graph showing the change in evaporation mass of the hydroelectric power generation device over time under 1.0 sun light intensity irradiation. The highest seawater evaporation rate can reach 2.75 kg / (m²). 2 *h). For example Figure 5 The graph shows the change of the interface evaporation temperature of the hydrovoltaic device over time under 1.0 sun light intensity. Within two minutes, the surface temperature can reach 120 degrees Celsius in dry conditions and 42 degrees Celsius in humid conditions, which means that the hydrogel phase transition temperature can be reached in humid conditions.
[0114] In this embodiment, the water sample was a simulated seawater solution (3.5 wt% NaCl), and the light source was 1.0 sun simulated sunlight. Figure 6 This refers to the maximum power output of a single hydroelectric power generation device after a one-hour test, as described in this example. The shaded area represents the output power, which is 23.33 uw / cm². 2 Electricity.
[0115] Example 3
[0116] In this embodiment, a wood-based hydrogel generator is provided, and its preparation method is as follows: A black porous wood board is processed into the shape of polyvinylidene fluoride (PVDF) aerogel as described in Example 1. The porous wood board is immersed in a dodecyl mercaptan ethanol solution (0.01 M) for 1 hour, and then the sample is dried in an oven (110 °C, 2 hours) to obtain a hydrophobically modified wood board. An NVCL-AMPS solution is prepared by dissolving 8 wt% N-vinylcaprolactam (NVCL), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 1 wt% 2-acrylamido-2-methylpropanesulfonic acid (AMPS) in deionized water. The porous wood board is then immersed in the NVCL solution, and the solution is subjected to vacuum filtration. The porous wood board filled with the hydrogel solution is cooled to 2-8 °C. Under a nitrogen atmosphere, the device is immersed in a 0.5 wt% tetramethylethylenediamine solution for 12 hours for crosslinking, allowing the internal hydrogel to crosslink in situ, resulting in NVCL-wood. Foamed stainless steel electrodes are embedded in porous wood. Two parallel foamed stainless steel electrodes are spaced 4 cm apart and embedded in the wood. The lower electrode is 2 cm away from the bottom. The foamed stainless steel electrodes are connected to an external energy harvesting device through wires to record the electrostatic energy generated inside the water-voltaic power generation device due to the separation of positive and negative ions in the solution.
[0117] In this embodiment, the water sample is a simulated seawater solution (3.5wt% NaCl), and the light source is 1.5sun simulated sunlight. Within 4 hours, the water-voltaic power generation device can generate a DC voltage output of about 0.1V. Figure 7 This refers to the hydrovolt power output of a single hydrovolt generator described in this example.
[0118] Example 4
[0119] In this embodiment, a foam-based hydrogel device is provided, and its preparation method is as follows: Black EVA foam is processed into the shape of polyvinylidene fluoride aerogel as described in Example 1, and chemical vapor deposition (90 °C, 2 h) is performed using vinyltrimethoxysilane (VTMO) to obtain hydrophobically modified EVA foam. A NAGA solution is prepared by dissolving 8 wt% N-acryloylglycine (NAGA), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 7 wt% dimethylaminoethyl methacrylate (DMAEMA) in deionized water. A porous wooden board is immersed in the NAGA solution, and the solution is subjected to vacuum filtration. The porous wooden board filled with the hydrogel solution is cooled to 2-8 °C. Under nitrogen atmosphere, the device is immersed in a 0.6 wt% tetramethylethylenediamine solution for crosslinking for 12 h, causing in-situ crosslinking of the internal hydrogel to obtain NAGA-EVA foam. The nickel foam electrodes are embedded in PNAGA-EVA foam. The two parallel nickel foam electrodes are set in wood with a 5cm gap between them. The lower electrode is 2cm away from the bottom. The nickel foam electrodes are connected to an external energy harvesting device through wires to record the electrostatic energy generated inside the water-voltaic power generation device due to the separation of positive and negative ions in the solution.
[0120] In this embodiment, the water sample is a simulated seawater solution (3.5wt% NaCl), and the light source is 1.0sun simulated sunlight. Within 4 hours, the water-voltaic power generation device can generate a DC voltage output of about 0.3V. Figure 8 This refers to the hydrovolt power output of a single hydrovolt generator described in this example.
[0121] As shown in Figures 7-8, the voltage values in Examples 3 and 4, which involve anionic modified hydrogels, are "positive". During the seawater evaporation process, the anionic modified hydrogels are electronegative, which promotes cation transport and hinders anion transport. A large number of cations accumulate at the upper electrode and a large number of anions accumulate at the lower electrode. During the test, the positive electrode of the external energy harvesting device is connected to the upper electrode and the negative electrode is connected to the lower electrode, thereby generating a positive potential difference.
[0122] Example 5
[0123] In this embodiment, a cellulose-based hydrovoltaic power generation device is provided, and its preparation method is as follows: 3 wt% graphene is dispersed in 1% TEMPO oxidized cellulose (TCNF). The above sol is poured into a unidirectional cryogenic mold. 4 cm × 2 cm foam copper electrodes are placed at a 7 cm interval between the top and bottom of the mold. Then, the mold is frozen in liquid nitrogen for 1 h and then freeze-dried for 24 h to obtain TCNF aerogel. Two parallel foam iron-nickel electrodes are spaced 7 cm apart and embedded in the aerogel, with the lower electrode and the bottom separated by 2 cm. The aerogel is immersed in diluted polydimethylsiloxane (PDMS) for 2 min, removed and cured. Then, the sample is subjected to chemical vapor deposition (80 °C, 2 h) with 1H, 1H, 2H, 2H-perfluorooctyltrichlorosilane (PFTOS) to obtain a hydrophobic TCNF aerogel (named TCPP). A PSPA solution was prepared by dissolving 8 wt% sebacic anhydride (SPA), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 10 wt% dimethylaminopropylacrylamide (DMAPAA) in deionized water. A cellulose aerogel was then immersed in the SPA solution, and the solution was subjected to vacuum filtration. The cellulose aerogel filled with the hydrogel solution was cooled to 2-8°C. Under nitrogen atmosphere, the device was immersed in a 0.55 wt% tetramethylethylenediamine solution for 12 hours to crosslink the internal hydrogel in situ, yielding a TCNF-PSPA aerogel. A copper foam electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0124] In this embodiment, the water sample is a simulated seawater solution (3.5wt% NaCl), and the light source is 1.0sun simulated sunlight. Within 4 hours, the water-voltaic power generation device can generate a DC voltage output of approximately -0.31V. Figure 9 This refers to the hydrovolt power output of a single hydrovolt generator described in this example.
[0125] Example 6
[0126] In this embodiment, a hydrogel-based photovoltaic device is provided, which is prepared as follows: Polyvinylidene fluoride (PVDF) is dissolved in dimethyl sulfoxide (DMSO) to prepare a 5wt% solution, and after stirring evenly, an aerogel solution is obtained. 10wt% graphite powder is dispersed into the aerogel solution, and 4cm × 2cm foamed stainless steel electrodes are placed vertically at a 2cm interval in a unidirectional cryogenic mold. The above sol is poured into the mold, then frozen in liquid nitrogen for 1 h, exchanged in a deionization environment at 2-8 degrees Celsius for 48 h, and then freeze-dried for 48 h to obtain polyvinylidene fluoride (PVDF) aerogel; wherein two parallel foamed stainless steel electrodes are spaced 2cm apart and embedded in the aerogel, with the lower electrode and the bottom separated by 2cm. A NIPAM-MPTAmC solution was prepared by dissolving 5 wt% N-isopropylacrylamide (NIPAM), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 1 wt% (3-acrylamidopropyl)trimethylammonium chloride (MPTAmC) in deionized water. The aerogel was then immersed in the NIPAM-MPTAmC solution and subjected to vacuum filtration. The aerogel filled with the hydrogel solution was cooled to 2-8°C. Under nitrogen atmosphere, the aerogel was then immersed in a 0.7% tetramethylethylenediamine solution for 12 hours to crosslink the hydrogel internally, resulting in a PVDF-PNIPAM-MPTAmC aerogel (named PPM). A foamed stainless steel electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0127] In this embodiment, the water sample is a simulated seawater solution (3.5wt% NaCl), and the light source is 1.0sun simulated sunlight. Within 4 hours, the water-voltaic power generation device can generate a DC voltage output of approximately -0.41V. Figure 10 This refers to the hydrovolt power output of a single hydrovolt generator described in this example.
[0128] As shown in Figures 9 and 10, Examples 5 and 6 both involve cationic modified hydrogels. During seawater evaporation, the cationic modified hydrogel is electropositive, which promotes anion transport and hinders cation transport, leading to the separation of positive and negative ions in the solution. A large number of anions accumulate at the upper electrode, and a large number of cations accumulate at the lower electrode. During the test, the positive electrode of the external energy harvesting device is connected to the upper electrode, and the negative electrode is connected to the lower electrode, thereby generating a negative potential difference.
[0129] Example 7
[0130] In this embodiment, a hydroelectric power generation device is provided, the preparation method of which is as follows: Poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) is dissolved in dimethyl sulfoxide to prepare a 5wt% solution, and after stirring evenly, an aerogel solution is obtained. 5wt% amorphous carbon is dispersed into the aerogel solution, and 4cm × 2cm foamed copper electrodes are placed vertically at a 5cm interval in a unidirectional cryogenic mold. The above sol is poured into the mold, then frozen in liquid nitrogen for 1 h, exchanged in a deionization environment at 2-8 degrees Celsius for 48 h, and then freeze-dried for 48 h to obtain poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) aerogel. Two parallel foamed copper electrodes are spaced 5cm apart and embedded in the center of the aerogel, with the lower electrode and bottom separated by a 2cm gap.
[0131] A PNIPAM-AMPS solution was prepared by dissolving 10 wt% N-isopropylacrylamide (NIPAM), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.5 wt% ammonium persulfate (APS), and 1 wt% 2-acrylamido-2-methylpropanesulfonic acid (AMPS) in deionized water. The aerogel was immersed in the PNIPAM-AMPS solution and then subjected to vacuum filtration. The aerogel filled with the hydrogel solution was cooled to 2-8°C. Under nitrogen atmosphere, the aerogel was immersed in a 5% tetramethylethylenediamine solution for 12 hours to crosslink the hydrogel internally, resulting in a PNIPAM-HFP-AMPS-PVDF aerogel (named PH-AP). A copper foam electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0132] In this embodiment, the water samples were deionized water, 3.5 wt% sodium chloride solution, 10 wt% sodium chloride solution, and 20 wt% sodium chloride solution, respectively. The light source was 1.0 sun simulated sunlight. Figure 11 This example illustrates the output of a water-based photovoltaic (VPC) generator in different solvents. When the water sample is deionized, the voltage initially rises and then falls due to the low ion count, reaching a maximum of 0.168V. As the ion concentration increases, the maximum output gradually increases, reaching 0.29V in a 3.5wt% sodium chloride solution and 0.325V in a 10wt% sodium chloride solution. With further increases in ion concentration, the high concentration at the bottom leads to a decrease in ion transport efficiency, resulting in a reduction in the maximum output.
[0133] Example 8
[0134] In this embodiment, a microcrystalline hydrovoltaic power generation device is provided, and its preparation method is as follows: 2.5g of microcrystalline cellulose (MCC) is added to 50g of a solution containing NaOH (7 wt%) and dimethyl sulfoxide (10 wt%). After the cellulose powder is completely dissolved, it is centrifuged (30min; 2500 rpm). A 4cm×2cm foam copper electrode is placed in a mold with a 3cm gap between the top and bottom. 5wt% graphene is added to the supernatant, and the resulting supernatant is poured into the mold for sol-gelation (5 h). After complete gelation, the gel material is washed with deionized water to obtain MCC hydrogel. Finally, the MCC hydrogel is subjected to rapid freezing and freeze-drying with liquid nitrogen (24 h) to obtain MCC aerogel. The two parallel upper and lower foam copper electrodes are spaced 3cm apart and embedded in the center of the aerogel, with the lower electrode and the bottom being 2cm apart.
[0135] A NIPAM-AMPS solution was prepared by dissolving 8 wt% N-isopropylacrylamide (NIPAM), 0.05 wt% N,N-methylenebisacrylamide (MBAA), 0.16 wt% ammonium persulfate (APS), and 2-acrylamido-2-methylpropanesulfonic acid (AMPS) in deionized water. The aerogel was immersed in the NIPAM-AMPS solution and subjected to vacuum filtration. The aerogel filled with the hydrogel solution was cooled to 2-8°C. Under nitrogen atmosphere, the aerogel was immersed in a 0.8 wt% tetramethylethylenediamine solution for 12 hours to crosslink, resulting in internal crosslinking of the hydrogel. This yielded an MCC-PNIPAM-AMPS aerogel (named MPA). A copper foam electrode was connected to an external energy harvesting device via wires to record the electrostatic energy generated inside the photovoltaic device due to the separation of positive and negative ions in the solution.
[0136] Figure 12 The images and ultraviolet spectra of the water quality before and after desalination by the hydrovoltaic power generation device described in this example demonstrate that the hydrovoltaic power generation device has the ability to desalinate water.
Claims
1. A gel composite material, characterized in that: The gel composite material has a hydrophobic insulating porous material as a skeleton, and the skeleton is filled with an ionic thermosensitive hydrogel; wherein the ionic thermosensitive hydrogel is a hydrogel modified with anionic groups or cationic groups; wherein the hydrogel modified with anionic groups or cationic groups is a crosslinked hydrogel of a cationic modifier or an anionic modifier and a matrix material, wherein the mass ratio of the matrix material to the ionic modifier in the ionic thermosensitive hydrogel is 10:1~1:1; The matrix material includes one or more of poly N-isopropylacrylamide PNIPAM, poly N-vinylcaprolactam PNVCL, polysebacic anhydride PSPA, and poly N-acryloylglycineamide PNAGA; the anion modifier includes at least one of 2-acrylamido-2-methylpropane sulfonic acid AMPS and dimethylaminoethyl methacrylate DMAEMA; the cationic modifier includes at least one of (3-acrylamidopropyl)trimethylammonium chloride MPTAmC and dimethylaminopropylacrylamide DMAPAA.
2. The gel composite material according to claim 1, characterized in that: The hydrophobic insulating porous material is a hydrophobic insulating porous material with a photothermal conversion function; the hydrophobic insulating porous material has vertically penetrating internal pores; The hydrophobic insulating porous material having a photothermal conversion function includes: a hydrophobic insulating porous material containing a photothermal functional filler or an intrinsic black hydrophobic insulating porous material without a photothermal functional filler; The photothermal functional filler includes one or more of carbon powder, carbon black, carbon nanotubes, graphene, graphite, amorphous carbon, MXene, metal organic framework MOF, and azobenzene; The mass percentage of the photothermal functional filler in the hydrophobic insulating porous material containing the photothermal functional filler is 1 wt % to 10 wt %.
3. The gel composite material according to claim 2, characterized in that: The hydrophobic insulating porous material containing photothermal functional fillers includes: one or more of aerogels, foam plastics, and porous wood containing photothermal functional fillers; The aerogel is one or more of unmodified aerogel, hydrophobic and / or insulating modified aerogel; the foam plastic is one or more of unmodified foam plastic, hydrophobic and / or insulating modified foam plastic; the porous wood is one or more of unmodified porous wood, hydrophobic and / or insulating modified porous wood.
4. The gel composite material according to claim 2, characterized in that: The intrinsic black hydrophobic insulating porous material without photothermal functional filler includes one or more of foam plastic and porous wood without photothermal functional filler; wherein the foam plastic is one or more of unmodified foam plastic and foam plastic modified by hydrophobicity and / or insulation; the porous wood is one or more of unmodified wood and porous wood modified by hydrophobicity and / or insulation.
5. The gel composite material according to any one of claims 3-4, characterized in that: The hydrophobic modification is one or more of surface micro-nano structure construction and surface hydrophobic coating processing; wherein the surface micro-nano structure construction method includes one or more of corrosion, etching, sol-gel method, and laser printing; wherein the surface hydrophobic coating processing includes one or more of surface coating and immersion treatment; wherein the material used for the surface hydrophobic coating processing includes one or more of fluorine-containing coating, silicon-containing coating, and fat chain-containing coating; The insulation modification is one or more of surface insulation treatment and impregnation insulation treatment; the material used for the insulation modification is at least one of organic insulation material, inorganic insulation material, and organic / inorganic composite insulation material; The organic insulating material is one or more of silicone resin, phenolic resin, epoxy resin, and polyimide; the inorganic insulating material is one or more of phosphate, silicate, TiO2, Cr2O3, MgO, ZrO2, SiO2, and Al2O3; the composite insulating material is one or more of SrTiO3 modified resin, SiO2 / SiC modified resin, Fe3O4 / SiO2 modified resin, and SiO2 modified resin.
6. A method for preparing the gel composite material according to any one of claims 1 to 4, comprising: (1) mixing a base monomer, a cross-linking agent, an initiator, a modifier, and a solvent to obtain a mixed solution; (2) The hydrophobic insulating porous material is immersed in the mixed solution, vacuum filtered, cooled, and then immersed in the catalyst solution under protective gas conditions for cross-linking to obtain a gel composite material.
7. The preparation method according to claim 6, characterized in that: In the step (1), the matrix monomer is one or more of N-isopropylacrylamide NIPAM, N-vinylcaprolactam NVCL, sebacic anhydride SPA, and N-acryloylglycineamide NAGA; the crosslinking agent is N,N-methylenebisacrylamide MBAA; the initiator is ammonium persulfate APS; the solvent is deionized water; and the modifier is a cationic modifier or an anionic modifier; In the mixed solution of step (1), the monomer accounts for 3wt% to 10wt% of the solvent by mass, the cross-linking agent accounts for 0.01wt% to 0.1wt% of the solvent by mass, the initiator accounts for 0.1wt% to 1wt% of the solvent by mass; and the modifier accounts for 0.3wt% to 10wt% of the solvent by mass; In the step (2), the temperature is cooled to 2-8° C.; the protective gas is nitrogen; the catalyst is tetramethylethylenediamine TEDMA; and the concentration of the catalyst solution is 0.5wt%~1wt%.
8. A hydroelectric power generation device, characterized in that: The hydrovoltaic power generation device comprises the gel composite material described in any one of claims 1 to 5 or the gel composite material prepared by the preparation method of the gel composite material described in any one of claims 6 to 7 and an electrode.
9. The hydrovoltaic power generation device according to claim 8, characterized in that: The electrodes include a positive electrode and a negative electrode; the gel composite material is provided with electrodes; wherein the positive electrode and the negative electrode are arranged in parallel; The electrode material is a porous electrode; wherein the porous electrode is a metal foam electrode or a graphite felt electrode; wherein the metal foam electrode includes one or more of a foam copper electrode, a foam stainless steel electrode, a foam iron-nickel electrode, a foam nickel electrode, a foam titanium electrode, and a foam aluminum electrode; The hydrovoltaic power generation device continuously outputs electrical energy during the evaporation process of the water body.
10. A method for preparing a hydrovoltaic power generation device according to any one of claims 8 to 9, comprising: Mixing a base monomer, a cross-linking agent, an initiator, a modifier, and a solvent to obtain a mixed solution; The hydrophobic insulating porous material is immersed in a mixed solution, vacuum filtered, cooled, and then immersed in a catalyst solution under protective gas conditions for cross-linking to obtain a gel composite material, and electrodes are assembled to obtain a hydrovoltaic power generation device; Or the matrix monomer, cross-linking agent, initiator, modifier and solvent are mixed to obtain a mixed solution; the hydrophobic insulating porous material equipped with electrodes is immersed in the mixed solution, vacuum filtered, cooled, and then immersed in a catalyst solution under protective gas conditions for cross-linking to obtain a hydrovoltaic power generation device.
11. Application of the hydrovoltaic power generation device according to any one of claims 8 to 9 or the hydrovoltaic power generation device prepared by the preparation method of the hydrovoltaic power generation device according to claim 10 in the fields of environment, new energy and renewable resources.
12. The use according to claim 11, characterized in that: The application in the environmental field includes one or more of seawater desalination, sewage treatment, distilled water collection, and plant bionic materials; The new energy field includes one or more of solar power generation and hydroelectric power generation; The renewable resource field includes one or more of plant growth monitoring, ecosystem services, ecosystem restoration, and water energy collection.
Citation Information
Patent Citations
Thermosensitive high strength and toughness nano-composite hydrogel and preparation method thereof
CN108794768A
Photo-thermal hydrogel, preparation method and application thereof, and photo-thermal conversion evaporator
CN114456308A
Hydrogel-based sponge solar seawater desalination material and preparation method thereof
CN116082698A
Preparation method of efficient atmospheric water vapor adsorption composite material
CN116571219A
Double-layer heterogeneous aerogel with moisture power generation and efficient solar water evaporation
CN118477578A