Method for purifying resin solution and purified resin solution
By combining the resin solution with high purity water and organic solvents, the problem of impurity of the resin solution is solved, the purification process is simplified, the amount of waste is reduced, and the performance of the liquid crystal display device is improved, and the raw liquid is realized A comparable resin solution purification effect.
Patent Information
- Application Number
- CN202310497631.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the used resin solution is difficult to meet the requirements of the liquid crystal display in terms of metal ion content, molecular weight distribution, viscosity and solid content, and the cumbersome recycling and processing process increases costs and generates additional waste.
By mixing the resin solution with high purity water to form a precipitate, the precipitate is then placed in the second organic solvent and then precipitated and dried, and finally filtered back to the solution and purified by precipitation, filtration and drying steps, it is suitable for different types of liquid crystal displays Device.
Simplified the purification process, significantly reduced the amount of waste, improved the performance of the liquid crystal display device, ensured the applicability and reliability of the purified resin solution on the liquid crystal display device, and reduced the metal ion weight to the stock solution level, viscosity and solid content Meets expected values.
Smart Images

Figure CN118895016A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for purifying a resin solution, in particular to a method for purifying a polyimide resin and a polyamic acid resin. Background Art
[0002] Because polyimide and polyamic acid are better than other organic polymers in terms of chemical stability, arrangement controllability, friction, etc., materials based on polyimide resin and polyamic acid resin are currently widely used as materials for liquid crystal arrangement of liquid crystal displays. The resin solution containing polyimide and polyamic acid used for liquid crystal arrangement should meet the requirements in terms of metal ion content, molecular weight distribution range, solid content, viscosity, etc. However, the used resin solution is impure and it is difficult to meet the requirements. In addition, in order to reduce the amount of waste, there is currently a practice of recycling and reusing the used resin solution. However, the cumbersome processing process and the use of consumables and liquid agents increase costs and also generate additional waste. Summary of the invention
[0003] The invention provides a method for purifying a resin solution, which is applicable to resin solutions of different types of liquid crystal display devices, has a simple process and significant effect, helps to reduce the amount of waste, and improves the problem of the performance degradation of liquid crystal display devices after use.
[0004] The resin solution purification method provided by the present invention comprises the following steps: providing a resin solution, which at least comprises polyimide, polyamic acid or a combination thereof, and a first organic solvent; providing high-purity water, placing the resin solution in the high-purity water for mixing, and forming a first precipitate; separating the first precipitate; providing a second organic solvent, placing the first precipitate in the second organic solvent for mixing, and forming a second precipitate; separating and drying the second precipitate; providing a solvent to dissolve the second precipitate and form a back solution, the solvent at least comprising the first organic solvent; filtering the back solution.
[0005] In one embodiment of the present invention, the step of mixing the resin solution and the high-purity water comprises mixing the resin solution and the high-purity water in a ratio of 1:1 to 1:20.
[0006] In one embodiment of the present invention, the ratio of the resin solution to high purity water is 1:3 to 1:10.
[0007] In one embodiment of the present invention, the ratio of the resin solution to high purity water is 1:4 to 1:8.
[0008] In one embodiment of the present invention, the step of mixing the first precipitate with the second organic solvent includes providing the second organic solvent in a ratio of 1:1 to 1:20 between the resin solution and the second organic solvent.
[0009] In one embodiment of the present invention, the step of mixing the first precipitate with the second organic solvent includes providing the second organic solvent in a ratio of 1:3 to 1:10 between the resin solution and the second organic solvent.
[0010] In one embodiment of the present invention, the step of mixing the first precipitate with the second organic solvent includes providing the second organic solvent in a ratio of 1:4 to 1:8 between the resin solution and the second organic solvent.
[0011] In one embodiment of the present invention, the first organic solvent includes N-methylpyrrolidone, ethylene glycol monobutyl ether, γ-butyrolactone or a combination thereof.
[0012] In one embodiment of the present invention, the second organic solvent includes methanol, ethanol, isopropanol, butanol, 2-butanol, ethylene glycol, alkanes or a combination thereof.
[0013] In one embodiment of the present invention, the step of separating the first precipitate includes filtering and separating using a metal filter; and the step of separating the second precipitate includes filtering and separating using a metal filter.
[0014] In one embodiment of the present invention, the step of drying the second precipitate includes drying the second precipitate in an environment below 30°C.
[0015] In one embodiment of the present invention, the step of filtering the solution back includes diluting the solution back with a solvent for filtering.
[0016] In one embodiment of the present invention, the step of filtering the solution back includes filtering using a filter membrane, and the pore size of the filter membrane is 0.1 micron-0.2 micron.
[0017] In one embodiment of the present invention, the step of filtering back the solution includes forming a filtrate, and the total amount of metal ions in the filtrate is not greater than 1 ppm.
[0018] In one embodiment of the present invention, the amount of any metal ion in the filtrate is less than 0.1 ppm.
[0019] In one embodiment of the present invention, the amount of the metal ions is 0 ppm.
[0020] The present invention also provides a purified resin solution prepared by the above steps.
[0021] The present invention adopts the steps of precipitation, filtration, drying, etc., so the method is simple and applicable to resin solutions of different types of liquid crystal display devices. The purified resin solution has a level equivalent to that of the original solution and has applicability and reliability in liquid crystal display devices.
[0022] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 FIG. 1 is a schematic flow chart of a method for purifying a resin solution according to an embodiment of the present invention. DETAILED DESCRIPTION
[0024] Unless otherwise clearly defined, the stock solution in the present disclosure is also called the resin stock solution, which is a resin solution that can be used in a liquid crystal display device and has not been used. The recovered liquid in the present disclosure is also called the resin recovered liquid or the recovered resin solution, which is a resin solution from a liquid crystal display device and used. The purified resin solution in the present disclosure can be a resin solution obtained by purifying the recovered liquid or the stock solution.
[0025] One embodiment of the present invention provides a method for purifying a resin solution, wherein the resin solution may be a material used for or derived from a liquid crystal display device, and further, may be a material used for liquid crystal arrangement in a liquid crystal display device. Preferably, the resin solution purified by the embodiment of the present invention contains polyimide, polyamic acid, or a combination thereof. The purification method of the embodiment of the present invention enables the viscosity and solid content of the resin solution to reach the expected values and meet the specifications. The purified resin solution is further tested by the electrical test of the liquid crystal box to confirm its applicability and reliability in the liquid crystal display device.
[0026] Please refer to Figure 1 , the purification method of an embodiment of the present invention includes steps S110-S170. Step S110: Provide a resin solution, which at least contains polyimide, polyamic acid or a combination thereof, and a first organic solvent. Step S120: Provide high-purity water, place the resin solution in the high-purity water for mixing, and form a first precipitate. Step S130: Separate the first precipitate. Step S140: Provide a second organic solvent, place the first precipitate in the second organic solution for mixing, and form a second precipitate. Step S150: Separate and dry the second precipitate. Step S160: Provide a solvent to dissolve the second precipitate and form a back solution, wherein the solvent at least contains the first organic solvent. Step S170: Filter the back solution.
[0027] The resin solution of step S110, in a preferred embodiment of the present invention, is a material for liquid crystal arrangement recovered from a liquid crystal display device. In addition to polyimide, polyamic acid, and the first organic solvent, the recovered resin solution is a used resin solution, and therefore usually contains other excess substances or the content of substances deviates from the acceptable range, resulting in impure resin recovery liquid, which affects its efficacy in the liquid crystal display device. For example, the amount of metal ions in the resin recovery liquid may exceed the standard value of the amount of metal ions in the resin stock solution. Excess small molecules in the recovery liquid are also one of the reasons for impurity. In addition, compared with the stock solution, the resin recovery liquid may deviate from the standard values in terms of water content, viscosity, solid content, etc.
[0028] The first organic solvent may vary depending on the type of the recovered resin solution, and may be a single organic solvent or a combination of multiple organic solvents. For example, the resin solution may be recovered from a vertical alignment (VA), in-plane switching (IPS) or twisted nematic (TN) liquid crystal display device, and thus, the resin recovery liquid may refer to a resin solution recovered from, for example, a VA, IPS, or TN liquid crystal display device. In some embodiments of the present invention, the first organic solvent includes, for example, N-methylpyrrolidone, ethylene glycol monobutyl ether, γ-butyrolactone, or a combination thereof.
[0029] The high-purity water in step S120 may be, for example, pure water. In an embodiment of the present invention, the high-purity water is preferably ultrapure water, and more preferably has a resistance value of less than 18M ohms. The ratio of the resin recovery liquid to the high-purity water is a weight ratio of 1:1-1:20, preferably 1:3-1:10, and more preferably 1:4-1:8. In some embodiments of the present invention, the mixing can be carried out in, for example, a stirring tank. In addition, the mixing can be further carried out in a temperature-controlled stirring tank such as a stainless steel material. After the recovery liquid and the high-purity water are fully mixed according to the ratio, a mixed liquid is formed. Step S120 includes standing the mixed liquid to wait for precipitation to occur, wherein polymers such as polyimide and polyamic acid are precipitated, and polymers such as polyimide and polyamic acid are the main components of the first precipitate. The standing time is preferably not more than 60 minutes. Other substances originally present in the recovery liquid include organic and inorganic molecules and ions, which can be dissolved or suspended in water in step S120.
[0030] The first precipitate in step S130 can be separated by, for example, filtering through a filter. The filter can have a filter screen, and the filter screen preferably has a pore size of 3-20 microns. If the filter screen is metal, it is preferably a material of SUS316 stainless steel or a titanium alloy or higher grade. In addition, the metal filter screen can be a porous metal material. In some embodiments of the present invention, a porous titanium metal filter screen is used to filter and separate the first precipitate. The separated first precipitate can be used in step S140.
[0031] In step S140, a second organic solvent within a certain weight range is provided to mix the first precipitate according to the amount of the recovered liquid in step S110. The weight ratio of the recovered liquid to the second organic solvent is 1:1-1:20, preferably 1:3-1:10, and more preferably 1:4-1:8. In some embodiments of the present invention, the second organic solvent may be, for example, methanol, ethanol, isopropanol, butanol, 2-butanol, ethylene glycol, alkanes or a combination thereof. The mixed solution is allowed to stand to allow precipitation to occur, wherein polymers such as polyimide and polyamic acid are precipitated, and polymers such as polyimide and polyamic acid are the main components of the second precipitate. Other substances originally present in the recovered liquid include organic and inorganic small molecules and ions, which can be dissolved or suspended in the second precipitate in step S140. In addition, the mixing in step S140 can also take away the moisture remaining in the first precipitate.
[0032] The separation of the second precipitate in step S150 can be performed with reference to step S130. The separated second precipitate can be dried naturally at room temperature, but preferably dried at an environment below 30 degrees Celsius. In some embodiments of the present invention, the drying can be performed in a vacuum oven, for example. The second precipitate can be in the form of a powder after drying. When the weight of the second precipitate after drying no longer changes, the drying is completed.
[0033] The solvent of step S160 can be provided according to the amount of the recovery solution in step S110. For example, the solvent can be provided according to the component volume ratio (i.e., the volume ratio of the solute to the solvent) of the recovery solution in step S110 until the recovery solution reaches the same solvent ratio as the recovery solution in step S110. The solvent used includes a first organic solvent. In some embodiments of the present invention, the recovery can be carried out in, for example, a temperature-controlled stirring tank.
[0034] In step S170, the solution can be filtered back using, for example, a filter membrane, and the filter membrane preferably has a pore size of 0.1 micron to 0.2 micron to further remove foreign matter with a particle size of 0.2 micron or more. The resin solution purified by steps S110-S170 can have the same content, viscosity, solid content, and physical and chemical properties as the original resin solution, and can be directly used in a liquid crystal display device. The present invention also evaluates the purified resin solution, as shown in Tables 1-5 and Examples 1-4 below.
[0035] Table 1: Evaluation items and equipment used for evaluation
[0036] Evaluation Project equipment Viscosity Viscometer Solid content Infrared moisture meter Metal ion content ICP-MS Voltage maintenance rate LCD Characteristics Tester Ion concentration LCD Characteristics Tester Afterimage Characteristics Spectrometer
[0037] In some embodiments of the present invention, each evaluation item may further adopt the following equipment: using a viscosity tester such as TOKISANGYO TVEL-25L, an infrared moisture meter such as METLER TOLEDO 204HX, an ICP-MS such as ICP350D, an LCD characteristic measuring instrument such as TOYO 6254, and a spectrometer such as Otsuka electronics LCD 5200.
[0038] Example 1: Physical and chemical properties of purified IPS liquid crystal display device resin solution
[0039] In this embodiment, the viscosity, solid content and metal ion content of the resin recovery liquid of the IPS type liquid crystal display device and the purified resin solution for the IPS type liquid crystal display device are evaluated and compared with the resin stock solution for the IPS type liquid crystal display device. The results are shown in Table 2.
[0040] Table 2:
[0041]
[0042] Table 2 shows that after the resin solution is purified, the viscosity, solid content, and metal ion content decrease, and are reduced to the viscosity, solid content, and metal ion content range of the resin stock solution, wherein the total amount of metal ions is not greater than 1ppm, and the amount of any metal ion is less than 0.1ppm. In some embodiments of the present invention, the amount of any metal ion can be less than 0.01ppm, and preferably reduced to 0.002ppm or less. Due to the decrease in viscosity, solid content, and metal ion content, it is obvious that the purified resin solution contains no or almost no other excess, and can be expected to have performance comparable to that of the resin stock solution.
[0043] Example 2: Electrical characteristics of a purified IPS liquid crystal display device resin solution
[0044] This embodiment evaluates the performance of the resin recovery liquid of the IPS type liquid crystal display device and the purified IPS type liquid crystal display device resin solution in the liquid crystal box, and compares it with the IPS type liquid crystal display device resin stock solution. The results are shown in Table 3.
[0045] Table 3:
[0046]
[0047]
[0048] Table 3 shows that after the IPS type resin solution is purified, its performance in voltage maintenance rate, ion concentration, afterimage, etc. can return to the level of the original resin solution.
[0049] Example 3: Physical and Chemical Properties of Purified TN Liquid Crystal Display Device Resin Solution
[0050] In this embodiment, the viscosity, solid content and metal ion content of the resin recovery liquid of the TN type liquid crystal display device and the purified resin solution for the TN type liquid crystal display device are evaluated and compared with the resin stock solution for the IPS type liquid crystal display device. The results are shown in Table 4.
[0051] Table 4:
[0052]
[0053] Table 4 shows that after the TN type resin solution is purified by the embodiments of the present invention, the viscosity, solid content, and metal ion content decrease, and are reduced to the viscosity, solid content, and metal ion content range of the resin stock solution, wherein the total amount of metal ions is not greater than 1ppm, and the amount of any metal ion is less than 0.1ppm. In some embodiments of the present invention, the amount of any metal ion can be less than 0.01ppm. Due to the decrease in viscosity, solid content, and metal ion content, it is obvious that the purified resin solution contains no or almost no other excess, and can be expected to have performance comparable to that of the resin stock solution.
[0054] Example 4: Electrical characteristics of a purified TN liquid crystal display device resin solution
[0055] This embodiment evaluates the performance of the resin recovery liquid of the TN type liquid crystal display device and the purified TN type liquid crystal display device resin solution in the liquid crystal box, and compares it with the TN type liquid crystal display device resin stock solution. The results are shown in Table 5.
[0056] Table 5:
[0057]
[0058]
[0059] Table 5 shows that after the TN type resin solution is purified, its performance in voltage holding rate, ion concentration, afterimage, etc. can return to the level of the original resin solution.
[0060] As can be seen from Examples 1-4, the purification method embodiments of the present invention are applicable to resin solutions of different types of liquid crystal display devices, so that the state of these resin solutions can be restored to a level equivalent to that of the original solution. Therefore, the problems of the liquid crystal display device caused by impure resin solution, such as reduced voltage hold ratio, increased ion density, and increased probability of image sticking, can be improved, and the amount of waste can be reduced.
[0061] The present disclosure also provides a purified resin solution, which is equivalent to the original solution in terms of viscosity, solid content, metal ion content, etc., and has the same level of the original solution in terms of voltage maintenance rate, ion concentration, afterimage, etc.
[0062] In an embodiment of the present invention, the purified resin solution provided comprises polyimide, polyamic acid or a combination thereof, and a first organic solvent. The first organic solvent comprises N-methylpyrrolidone, ethylene glycol monobutyl ether, γ-butyrolactone or a combination thereof. Further, the purified resin solution may be, for example, a purified IPS-type liquid crystal display device resin solution, a purified TN-type liquid crystal display device resin solution. In some embodiments, the purified IPS-type liquid crystal display device resin solution may have a viscosity of 15-65mPas and a solid content of 3.5-9.0%, and preferably, a viscosity of 35-50mPas and a solid content of 4-8%. In some embodiments, the purified TN-type liquid crystal display device resin solution may have a viscosity of 15-70mPas and a solid content of 4-8%, and preferably, a viscosity of 15-35mPas and a solid content of 4-7.5%. The purified resin solution of the present invention is preferably prepared by the aforementioned steps S110-S170. In the purified resin solution provided by the embodiment of the present invention, the total amount of metal ions may be no greater than 1 ppm, and the amount of any one metal ion may be less than 0.1 ppm.
[0063] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A method for purifying a resin solution, It is characterized in that include: Providing a resin solution, wherein the resin solution at least comprises polyimide, polyamic acid or a combination thereof, and a first organic solvent; Providing high-purity water, placing the resin solution into the high-purity water for mixing, and forming a first precipitate; separating the first precipitate; Providing a second organic solvent, placing the first precipitate into the second organic solvent for mixing, and forming a second precipitate; separating and drying the second precipitate; Providing a solvent to dissolve the second precipitate and form a back solution, wherein the solvent at least comprises the first organic solvent; and The solution was filtered.
2. The method for purifying a resin solution according to claim 1, It is characterized in that The step of mixing the resin solution with the high-purity water includes mixing the resin solution with the high-purity water in a ratio of 1:1 to 1:
20.
3. The method for purifying a resin solution according to claim 2, It is characterized in that The ratio of the resin solution to the high purity water is 1:3 to 1:
10.
4. The method for purifying a resin solution according to claim 3, It is characterized in that The ratio of the resin solution to the high purity water is 1:4 to 1:
8.
5. The method for purifying a resin solution according to claim 1, It is characterized in that The step of mixing the first precipitate with the second organic solvent includes providing the second organic solvent according to a ratio of 1:1 to 1:20 between the resin solution and the second organic solvent.
6. The method for purifying a resin solution according to claim 5, It is characterized in that The second organic solvent is provided according to a ratio of the resin solution to the second organic solvent of 1:3 to 1:
10.
7. The method for purifying a resin solution according to claim 6, It is characterized in that The second organic solvent is provided according to a ratio of the resin solution to the second organic solvent of 1:4 to 1:
8.
8. The method for purifying a resin solution according to claim 1, It is characterized in that The first organic solvent includes N-methylpyrrolidone, ethylene glycol monobutyl ether, γ-butyrolactone or a combination thereof.
9. The method for purifying a resin solution according to claim 1, It is characterized in that The second organic solvent includes methanol, ethanol, isopropanol, butanol, 2-butanol, ethylene glycol, alkanes or a combination thereof.
10. The method for purifying a resin solution according to claim 1, It is characterized in that The step of separating the first precipitate includes filtering and separating by using a metal filter; and the step of separating the second precipitate includes filtering and separating by using a metal filter.
11. The method for purifying a resin solution according to claim 1, It is characterized in that The step of drying the second precipitate includes drying the second precipitate in an environment below 30°C.
12. The method for purifying a resin solution according to claim 1, It is characterized in that The step of filtering the back solution includes diluting the back solution with the solvent to perform the filtering.
13. The method for purifying a resin solution according to claim 1, It is characterized in that The step of filtering the solution includes filtering with a filter membrane, and the pore size of the filter membrane is 0.1 micron-0.2 micron.
14. The method for purifying a resin solution according to claim 1, It is characterized in that The step of filtering the back solution includes forming a filtrate, and the total amount of metal ions in the filtrate is not greater than 1 ppm.
15. The method for purifying a resin solution according to claim 14, It is characterized in that The amount of any metal ion in the filtrate is less than 0.1 ppm.
16. The method for purifying a resin solution according to claim 15, It is characterized in that The amount of this metal ion is 0 ppm.
17. A purified resin solution, It is characterized in that Prepared by the following steps: Providing a recycled resin solution, wherein the recycled resin solution at least comprises polyimide, polyamic acid or a combination thereof, and a first organic solvent; Providing high-purity water, placing the recovered resin solution into the high-purity water for mixing, and forming a first precipitate; separating the first precipitate; Providing a second organic solvent, placing the first precipitate into the second organic solvent for mixing, and forming a second precipitate; separating and drying the second precipitate; Providing a solvent to dissolve the second precipitate and form a back solution, wherein the solvent at least comprises the first organic solvent; and The solution was filtered.
18. The purified resin solution of claim 17, It is characterized in that The purified resin solution has a viscosity of 15-70 mPas and a solid content of 3.5-9.0%.
19. The purified resin solution of claim 17, It is characterized in that The first organic solvent includes N-methylpyrrolidone, ethylene glycol monobutyl ether, γ-butyrolactone or a combination thereof.
20. The purified resin solution of claim 17, It is characterized in that The purified resin solution has a total amount of metal ions of no greater than 1 ppm.