High-barrier nano polyvinyl alcohol composite material and preparation method thereof
By using raw materials such as phosphogypsum, water, PVA resin, nanomontmorillonite and other raw materials in PVA packaging film, the layered structure of nanomontmorillonite extends the diffusion route of gas and water molecules, PVA is solved by using the layered structure of nanomontmorillonite. The problem of high moisture permeability of the packaging film in humid environments achieves high oxygen resistance and high water resistance, and facilitates melt processing.
Patent Information
- Application Number
- CN202410890256.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-05
AI Technical Summary
The existing PVA packaging film has high moisture permeability in humid environments, resulting in low water vapor barrier performance and is unable to have both high gas barrier and high water barrier properties.
The emulsion is formed by using phosphogypsum, water, PVA resin, nanomontmorillonite, dispersant, concentrated sulfuric acid, concentrated nitric acid and other raw materials, and the emulsion is formed by uniform mixing and sufficient reaction. After filtering, washing and drying, it is mixed with antioxidants and polyethylene wax. Extrusion and granulation are formed to form nanopolyvinyl alcohol composite materials, and the layered structure of nanomontmorillonite is used to extend the diffusion route of gas and water molecules, increasing oxygen and water resistance.
The high oxygen resistance and water resistance of the composite material are achieved, and the melting point of PVA macromolecules is reduced, which is convenient for melt processing and maintains the transparency of the material.
Smart Images

Figure CN118895032A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a high-barrier nano-polyvinyl alcohol composite material and a preparation method thereof. Background Art
[0002] PVA packaging film products are green and environmentally friendly materials. They are biodegradable polymer materials that are non-toxic, odorless, harmless, and have good affinity with the natural environment. PVA film has excellent oxygen barrier properties under dry conditions, and its oxygen permeability coefficient is the lowest among various resin films. PVA film has strong permeability to moisture and ammonia, but has excellent barrier properties to oxygen, nitrogen, hydrogen, helium, argon and carbon dioxide. The barrier rate to oxygen under normal pressure is about 1000 times that of commonly used polyethylene film and 300 times that of polypropylene film. The use of PVA film can keep the ingredients and smell of the packaged product intact. However, the moisture permeability of PVA packaging film is very high. It is a film with extremely high moisture permeability. It has extremely low water vapor barrier performance and high hygroscopicity, which makes it easy to soak the packaged product in a humid environment or the wet packaged product is easy to leak water to the outside of the packaging film. Therefore, it is urgent to prepare a PVA material with both high gas barrier properties and high water barrier properties. Summary of the invention
[0003] The purpose of the present invention is to provide a high-barrier nano-polyvinyl alcohol composite material having both high gas barrier properties and high water barrier properties and a preparation method thereof in view of the above-mentioned problems existing in the prior art.
[0004] To achieve the above objectives, the technical solution of the present invention is as follows:
[0005] In the first aspect, the present invention provides a high-barrier nano-polyvinyl alcohol composite material, the raw materials of the composite material comprising: a composite masterbatch and auxiliary materials; wherein the raw materials of the composite masterbatch comprise: phosphogypsum, water, PVA resin, nano-montmorillonite, a dispersant, concentrated sulfuric acid, and concentrated nitric acid.
[0006] The mass ratio of the phosphogypsum, water, PVA resin, nano-montmorillonite, dispersant, concentrated sulfuric acid and concentrated nitric acid is 80-100:1600-2000:80-100:10-20:3-5:8-10:8-10.
[0007] The mass ratio of the composite masterbatch to the auxiliary materials is 80-100:0.4-0.7.
[0008] The dispersant is sodium dodecylbenzene sulfonate; the auxiliary materials include antioxidants and polyethylene wax.
[0009] The mass ratio of the composite masterbatch, antioxidant and polyethylene wax is 80-100:0.1-0.2:0.3-0.5.
[0010] In a second aspect, the present invention provides a method for preparing a high barrier nano-polyvinyl alcohol composite material, the preparation method comprising:
[0011] The first step is to uniformly mix phosphogypsum and water in a required proportion, then add PVA resin, nano-montmorillonite and dispersant in a required proportion and mix them evenly, then add concentrated sulfuric acid and concentrated nitric acid in a required proportion, and fully react at 90-100° C. After the reaction is completed, an emulsion is obtained, and the emulsion is filtered while hot to obtain a filtrate. After the filtrate is cooled to room temperature, the filtrate is filtered, washed and dried in sequence to obtain a composite masterbatch;
[0012] The second step is to mix the composite masterbatch and the auxiliary materials in the required proportion and then extrude and granulate them to obtain a high barrier nano-polyvinyl alcohol composite material.
[0013] The mass ratio of the phosphogypsum, water, PVA resin, nano-montmorillonite, dispersant, concentrated sulfuric acid and concentrated nitric acid is 80-100:1600-2000:80-100:10-20:3-5:8-10:8-10.
[0014] The mass ratio of the composite masterbatch to the auxiliary materials is 80-100:0.4-0.7.
[0015] The dispersant is sodium dodecylbenzene sulfonate; the auxiliary materials include antioxidants and polyethylene wax; the mass ratio of the composite masterbatch, antioxidant AT-76 and polyethylene wax is 80-100:0.1-0.2:0.3-0.5.
[0016] The extrusion granulation is carried out in a twin-screw extruder, and the extrusion process temperature of the twin-screw extruder is: 175±5°C in zone one, 180±5°C in zone two, 190±5°C in zone three, 200±5°C in zone four, 210±5°C in zone five, 215±5°C in zone six, 220±5°C in zone seven, 215±5°C in zone eight, 200±5°C in zone nine, and 200±5°C in the die head.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The invention discloses a preparation method of a high-barrier nano-polyvinyl alcohol composite material, comprising the following steps: firstly, phosphogypsum and water are uniformly mixed in a required proportion, then PVA resin, nano-montmorillonite and a dispersant are added in a required proportion and mixed evenly, then concentrated sulfuric acid and concentrated nitric acid are added in a required proportion, and the mixture is fully reacted at 90-100° C. After the reaction is completed, an emulsion is obtained, the emulsion is filtered while hot to obtain a filtrate, and the filtrate is cooled to room temperature, and the filtrate is filtered, washed and dried in sequence to obtain a composite masterbatch; finally, the composite masterbatch and auxiliary materials are uniformly mixed in a required proportion, and then extruded and granulated to obtain a high-barrier nano-polyvinyl alcohol composite material. Nano-montmorillonite composite material; the nano-montmorillonite added in this design has a layered structure. Gas molecules and water molecules cannot pass through the layers and must diffuse in the gaps between the layers. This greatly extends the route for gas passage, so that the composite material has excellent oxygen and water barrier properties. The barrier properties are enhanced with the increase of the content of nano-montmorillonite. Under normal circumstances, it is difficult for polymer PVA macromolecules to enter the layer structure of montmorillonite and cannot form a true nano-intercalation material. This design first dissolves PVA resin and nano-montmorillonite. In an aqueous solution containing phosphogypsum, the calcium sulfate molecules in the phosphogypsum can enter the nano-montmorillonite lamellar structure, and then generate calcium sulfate whiskers in the nano-montmorillonite lamellar structure in the presence of concentrated sulfuric acid and concentrated nitric acid, which expands the interlayer spacing of the nano-montmorillonite lamellar structure, so that the polymer PVA macromolecules can be smoothly inserted into the montmorillonite silicate lamellae, forming a true PVA polymer nano-intercalation composite material; although the interlayer spacing of the nano-montmorillonite lamellae is expanded due to the insertion of calcium sulfate whiskers and polymer macromolecules, there is still a gap between the nano-montmorillonite lamellae. Under strong van der Waals forces, the arrangement between the layers is still regular and orderly, and the layer structure of the nano-montmorillonite will not be destroyed, so the oxygen barrier and water barrier properties of the composite material will not be reduced; in addition, since polyvinyl alcohol is a crystalline polymer, the molecule contains a large number of hydroxyl groups, and there are a large number of hydrogen bonds between molecules, it is difficult to plasticize and melt-process. This design separates the PVA macromolecules through the montmorillonite layer, thereby preventing the formation of hydrogen bonds between the PVA macromolecules and limiting their crystallization, thereby reducing their melting point, which is beneficial to the melt processing of the composite material. Therefore, the composite material of the present invention has high oxygen barrier and high water barrier properties, and has a low melting point, which is convenient for melt processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the composite material obtained in Example 1.
[0020] Figure 2 Schematic diagram of the composite material obtained in Comparative Example 2.
[0021] Calcium sulfate whiskers are not shown in the figure. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below in conjunction with specific implementations and drawings.
[0023] The present invention aims to design a nano-polyvinyl alcohol composite material with high oxygen barrier and high water barrier. The added nano-montmorillonite is of nanometer size, which is smaller than the wavelength of visible light, and the light wave can bypass the sheet layer. Therefore, the addition of nano-montmorillonite does not affect the transparency of the composite material. The material can be used for the production of PVA packaging film.
[0024] Phosphogypsum: industrial grade;
[0025] PVA resin: PVA1799, white solid powder, average degree of polymerization is about 1700, alcoholysis degree is 99%;
[0026] Nano-montmorillonite: purchased from Zhejiang Fenghong New Materials Co., Ltd., purity ≥99%, average particle size 50-80nm;
[0027] Sodium dodecylbenzene sulfonate: surfactant, dispersant;
[0028] Concentrated sulfuric acid: industrial grade;
[0029] Concentrated nitric acid: industrial grade;
[0030] Antioxidant AT-76: white crystalline powder, anti-heat aging agent;
[0031] Polyethylene wax: white flakes.
[0032] Embodiment 1:
[0033] A nano polyvinyl alcohol composite material comprises 80 kg of composite masterbatch, 0.1 kg of antioxidant AT-76 and 0.3 kg of polyethylene wax; the composite masterbatch comprises 80 kg of phosphogypsum, 1600 kg of distilled water, 80 kg of PVA resin (powder), 10 kg of nano montmorillonite, 3 kg of sodium dodecylbenzene sulfonate, 8 kg of concentrated sulfuric acid and 8 kg of concentrated nitric acid.
[0034] The preparation method of the nano-polyvinyl alcohol composite material is specifically carried out according to the following steps:
[0035] The first step is to add phosphogypsum and distilled water into the reactor in the required proportion and stir at a stirring speed of 200 rpm and a heating temperature of 90°C; then add PVA resin, nano-montmorillonite and dispersant in the required proportion and perform ultrasonic dispersion for 10 minutes; then add concentrated sulfuric acid and concentrated nitric acid in the required proportion and react at 90°C for 15 minutes. After the reaction is completed, an emulsion is obtained, and the filtrate is filtered while hot to obtain a filtrate. After the filtrate is cooled to room temperature, the filtrate is filtered, washed and dried in sequence to obtain a composite masterbatch; wherein the dispersant is sodium dodecylbenzene sulfonate, and the phosphogypsum is pretreated phosphogypsum, and the pretreatment is: grinding the phosphogypsum in a ball mill for 15 minutes, and filtering the ground phosphogypsum through an 800-mesh sieve;
[0036] The second step is to add the composite masterbatch, antioxidant AT-76 and polyethylene wax into a high-speed mixer in the required proportion, mix at room temperature for 10 minutes, and then discharge the obtained mixture into a parallel twin-screw extruder granulator, melt-blending, extrusion and granulation to obtain a high-barrier nano-polyvinyl alcohol composite material; wherein the extrusion process temperature of the twin-screw extruder is: 175±5℃ for zone 1, 180±5℃ for zone 2, 190±5℃ for zone 3, 200±5℃ for zone 4, 210±5℃ for zone 5, 215±5℃ for zone 6, 220±5℃ for zone 7, 215±5℃ for zone 8, 200±5℃ for zone 9, and 200±5℃ for the die.
[0037] Embodiment 2:
[0038] The difference from Example 1 is that:
[0039] The addition amounts of the composite masterbatch, antioxidant and polyethylene wax are 100kg, 0.2kg and 0.5kg respectively;
[0040] The addition amounts of the phosphogypsum, distilled water, PVA resin, nano-montmorillonite, sodium dodecylbenzene sulfonate, concentrated sulfuric acid and concentrated nitric acid are 100kg, 2000kg, 100kg, 20kg, 5kg, 10kg and 10kg respectively;
[0041] The reaction temperature is 100°C.
[0042] Embodiment 3:
[0043] The difference from Example 1 is that:
[0044] The addition amounts of the composite masterbatch, antioxidant and polyethylene wax are 90kg, 0.15kg and 0.4kg respectively;
[0045] The added amounts of the phosphogypsum, distilled water, PVA resin, nano-montmorillonite, sodium dodecylbenzene sulfonate, concentrated sulfuric acid and concentrated nitric acid are 90kg, 1800kg, 90kg, 15kg, 4kg, 9kg and 9kg respectively.
[0046] The reaction temperature was 95°C.
[0047] Embodiment 4:
[0048] The difference from Example 1 is that:
[0049] The addition amounts of the composite masterbatch, antioxidant and polyethylene wax are 95kg, 0.2kg and 0.4kg respectively;
[0050] The added amounts of the phosphogypsum, distilled water, PVA resin, nano-montmorillonite, sodium dodecylbenzene sulfonate, concentrated sulfuric acid and concentrated nitric acid are 95kg, 1900kg, 95kg, 8kg, 4kg, 9kg and 9kg respectively.
[0051] Embodiment 5:
[0052] The difference from Example 1 is that:
[0053] The addition amounts of the composite masterbatch, antioxidant and polyethylene wax are 100kg, 0.2kg and 0.5kg respectively;
[0054] The added amounts of the phosphogypsum, distilled water, PVA resin, nano-montmorillonite, sodium dodecylbenzene sulfonate, concentrated sulfuric acid and concentrated nitric acid are 80kg, 1700kg, 80kg, 10kg, 4kg, 9kg and 10kg respectively.
[0055] Performance Verification:
[0056] In order to verify the effectiveness of the composite material of the present invention, the oxygen barrier performance and water barrier performance of Comparative Example 1, Comparative Example 2 and Test Example were tested respectively; the test example is the composite material prepared in Example 1, Comparative Example 1 is a commercially available PVA ordinary film (purchased from Zhengzhou Green Voice Packaging Material Co., Ltd.), Comparative Example 2 is a composite material prepared with other masterbatches (the masterbatch is obtained by mixing calcium sulfate whiskers, nano-montmorillonite and PVA resin, and the preparation steps of the composite material are the same as the second step of Example 1), and Comparative Example 3 is a commercially available BOPP film; the test method for oxygen barrier performance specifically refers to GB / T1038-2022 Test method for gas permeability of plastic films and sheets, and the test method for water barrier performance specifically refers to GB / T1037-2021 Cup weight gain and weight loss method for water vapor permeability of plastic films and sheets; the test results are shown in Table 1:
[0057] Table 1 Oxygen barrier properties and water barrier properties
[0058] Product Name Oxygen barrier Water barrier (water vapor transmission rate) Comparative Example 1 <![CDATA[8cm 3 / (m 2 ·24h·0.1MPa)]]> <![CDATA[32g / (m 2 ·24h·0.1MPa)]]> Comparative Example 2 <![CDATA[6cm 3 / (m 2 ·24h·0.1MPa)]]> <![CDATA[26(m 2 ·24h·0.1MPa)]]> Comparative Example 3 <![CDATA[625cm 3 / (m 2 ·24h·0.1MPa)]]> <![CDATA[35(m 2 ·24h·0.1MPa)]]> Test Case <![CDATA[0.1cm 3 / (m 2 ·24h·0.1MPa)]]> <![CDATA[1g / m 2 ·24h·0.1MPa)]]>
[0059] As shown in Table 1, the oxygen barrier performance and water barrier performance of the test example are significantly better than those of comparative example 1 and comparative example 2. This is because the nano-montmorillonite in comparative example 2 is dispersed in the polymer matrix like a filler material, and the PVA macromolecules do not enter the nano-montmorillonite interlayer structure (such as Figure 2 As shown), it cannot form a nano-intercalation material, but can only form a common blended material, and the common blended material does not have high barrier properties, and therefore does not have high oxygen barrier properties and high water barrier properties. After the interlayer spacing of the nano-montmorillonite of Example 1 is enlarged by the calcium sulfate whiskers, the PVA macromolecules can be inserted into the montmorillonite layer (as shown in Figure 1 As shown), a true PVA polymer nano-intercalation composite material is formed, which greatly improves the barrier performance; the melting point of the composite material obtained in Example 1 is 190°C, which is 40°C lower than the melting point of 230°C of the PVA resin (purchased from Shanghai Petrochemical, PVA1788).
Claims
1. A high barrier nano polyvinyl alcohol composite material, characterized in that: The raw materials of the composite material include: composite masterbatch and auxiliary materials; wherein the raw materials of the composite masterbatch include: phosphogypsum, water, PVA resin, nano-montmorillonite, dispersant, concentrated sulfuric acid and concentrated nitric acid.
2. The high barrier nano-polyvinyl alcohol composite material according to claim 1, characterized in that: The mass ratio of the phosphogypsum, water, PVA resin, nano-montmorillonite, dispersant, concentrated sulfuric acid and concentrated nitric acid is 80-100:1600-2000:80-100:10-20:3-5:8-10:8-10.
3. A high barrier nano-polyvinyl alcohol composite material according to claim 1 or 2, characterized in that: The mass ratio of the composite masterbatch to the auxiliary materials is 80-100:0.4-0.
7.
4. A high barrier nano-polyvinyl alcohol composite material according to claim 1 or 2, characterized in that: The dispersant is sodium dodecylbenzene sulfonate; the auxiliary materials include antioxidants and polyethylene wax.
5. The high barrier nano-polyvinyl alcohol composite material according to claim 4, characterized in that: The mass ratio of the composite masterbatch, the antioxidant and the polyethylene wax is 80-100:0.1-0.2:0.3-0.
5.
6. A method for preparing a high barrier nano-polyvinyl alcohol composite material, characterized in that: The preparation method comprises: The first step is to uniformly mix phosphogypsum and water in a required proportion, then add PVA resin, nano-montmorillonite and dispersant in a required proportion and mix them evenly, then add concentrated sulfuric acid and concentrated nitric acid in a required proportion, and fully react at 90-100° C. After the reaction is completed, an emulsion is obtained, and the emulsion is filtered while hot to obtain a filtrate. After the filtrate is cooled to room temperature, the filtrate is filtered, washed and dried in sequence to obtain a composite masterbatch; The second step is to mix the composite masterbatch and the auxiliary materials in the required proportion and then extrude and granulate them to obtain a high barrier nano-polyvinyl alcohol composite material.
7. The method for preparing a high barrier nano-polyvinyl alcohol composite material according to claim 6, characterized in that: The mass ratio of the phosphogypsum, water, PVA resin, nano-montmorillonite, dispersant, concentrated sulfuric acid and concentrated nitric acid is 80-100:1600-2000:80-100:10-20:3-5:8-10:8-10.
8. The method for preparing a high barrier nano-polyvinyl alcohol composite material according to claim 6 or 7, characterized in that: The mass ratio of the composite masterbatch to the auxiliary materials is 80-100:0.4-0.
7.
9. The method for preparing a high barrier nano-polyvinyl alcohol composite material according to claim 6 or 7, characterized in that: The dispersant is sodium dodecylbenzene sulfonate; the auxiliary materials include antioxidants and polyethylene wax; the mass ratio of the composite masterbatch, antioxidant AT-76 and polyethylene wax is 80-100:0.1-0.2:0.3-0.
5.
10. The method for preparing a high barrier nano-polyvinyl alcohol composite material according to claim 6 or 7, characterized in that: The extrusion granulation is carried out in a twin-screw extruder, and the extrusion process temperature of the twin-screw extruder is: 175±5°C in zone one, 180±5°C in zone two, 190±5°C in zone three, 200±5°C in zone four, 210±5°C in zone five, 215±5°C in zone six, 220±5°C in zone seven, 215±5°C in zone eight, 200±5°C in zone nine, and 200±5°C in the die head.