Multi-layer high-barrier film as well as preparation method and application thereof
Through the coextrusion process and the blend of POE-g-MAH, POE-g-GMA and tackifying resin as the adhesive layer, the problem of poor adhesion of polyglycolic acid in multilayer films was solved, and high efficiency was prepared. Degradable high-barrier film with excellent water and oxygen resistance properties.
Patent Information
- Application Number
- CN202310606402.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, when preparing high barrier multilayer films, the processing temperature of polyglycolic acid is high, the toughness is poor, and the adhesion force with other resins is poor, resulting in limited improvement in barrier performance and complex process and low efficiency.
Using co-extrusion process, pure polyglycolic acid is used as the barrier layer, and the blend of POE-g-MAH, POE-g-GMA and tackifying resin is used as the adhesive layer to improve the polyethylene and polyglycolic acid. Adhesion problem, a high barrier film without layering was prepared.
It realizes an efficient and degradable multi-layer film, with excellent water and oxygen resistance properties, and improves the adhesion between polyglycolic acid and other layers, improving production efficiency.
Smart Images

Figure BDA0004250707510000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of multilayer films, and in particular relates to a multilayer high-barrier film and a preparation method and application thereof. Background Art
[0002] Polyglycolic acid (PGA for short) is an aliphatic polyester polymer material with the least carbon unit number, a completely decomposable ester structure, and the fastest degradation rate. It eventually decomposes into water and carbon dioxide. It is a material recognized by the world to protect the earth's environment and life. Polyglycolic acid has excellent biocompatibility, mechanical strength, and excellent gas barrier properties. Its barrier properties to oxygen and water vapor are 100 times that of PET and 1000 times that of PLA, and PGA's barrier properties to gases are basically unaffected by ambient temperature. Therefore, placing the PGA component in the core layer of a multi-layer film as a barrier layer is an ideal material choice for multi-layer barrier films and can be used to develop new multi-layer degradable films.
[0003] However, due to the high processing temperature, poor toughness, and poor adhesion of PGA with other resins, its use in high-barrier films to improve barrier properties is limited, and there are few studies and reports on related improvement plans.
[0004] Patent document CN113232395A discloses a fully biodegradable composite film material with barrier properties and its packaging bag. The composite film material includes a cellulose layer, a PGA layer, a PBAT layer, a first adhesive layer sandwiched between the PBAT layer and the PGA layer, and a second adhesive layer between the PGA layer and the cellulose layer from top to bottom. The PBAT layer, the first adhesive layer, the PGA layer, the second adhesive layer and the cellulose layer are combined together by composite film forming technology. The invention combines a cellulose layer with printing adaptability but poor extensibility and no heat sealability with a PGA with barrier properties through a second adhesive layer, and then combines it with a PBAT layer with heat sealability and extensibility through a first adhesive layer. The properties of the two are complementary, and a composite film material with good surface wetting tension, heat resistance and heat sealability, adaptability to low-temperature freezing, and certain barrier properties can be made. Most of the materials are derived from degradable raw materials, which is green and environmentally friendly. However, this patent uses a hot pressing molding process, which is complex and inefficient.
[0005] Patent document CN105793040A discloses a polymer mixture for barrier film, the biodegradable polyester mixture comprising: i) 55 to 90 weight % of polyglycolic acid (PGA) relative to components i) and ii), and ii) 10 to 45 weight % of biodegradable polyester relative to components i) and ii), which is formed by aliphatic or aliphatic and aromatic dicarboxylic acids and aliphatic diols. The invention also relates to a single-layer or multi-layer film comprising the polymer mixture, and the use of the film for packaging food. However, each layer of this patent is a mixture of PGA and degradable polyester, and there is no pure PGA layer, so the improvement of barrier properties is affected.
[0006] Patent document CN114434929A discloses a degradable film for disposable bags for biopharmaceuticals and its application. The film includes five layers from the outside to the inside, namely, a protective layer, a first adhesive layer, a high barrier layer, a second adhesive layer and a liquid contact layer; the protective layer is PBAT:PBS:PGA=(40-70):(10-40):(5-30), the first adhesive layer and the second adhesive layer are made of adhesive resin; the high barrier layer is made of fully biodegradable vinyl alcohol copolymer; the liquid contact layer is made of linear low-density polyethylene modified with biodegradable filler; there is no pure PGA layer in the film, and the PVA layer mainly plays a barrier role, because the PVA as a barrier layer is water-soluble, and the barrier property is greatly affected by temperature and humidity.
[0007] In view of this, continuing to develop multilayer films with high barrier properties and their preparation methods has become a direction worthy of research. Summary of the invention
[0008] The purpose of the present invention is to provide a multi-layer high barrier film and its preparation method and application in view of the shortcomings of the prior art in preparing high barrier multi-layer films. The co-extrusion process is adopted, and the barrier layer in the multi-layer film is pure polyglycolic acid (PGA). On the basis of improving the bonding problem between polyethylene and polyglycolic acid, a non-stratified high barrier film can be prepared, and the multi-layer film is degradable and has excellent water barrier and oxygen barrier properties.
[0009] In order to achieve the above object, the present invention provides the following technical solutions:
[0010] In a first aspect, a multi-layer high barrier film is provided, the multi-layer high barrier film comprising: an outer layer / adhesive layer / barrier layer / adhesive layer / outer layer arranged in sequence; wherein:
[0011] The outer layer is polyethylene;
[0012] The adhesive layer is selected from POE-g-MAH, POE-g-GMA, a blend of POE-g-MAH and a tackifying resin, and a blend of POE-g-GMA and a tackifying resin;
[0013] The barrier layer is polyglycolic acid.
[0014] According to the multilayer high barrier film provided by the present invention, in one embodiment, the polyethylene has a melt index of 1.0 to 10.0 g / 10 min (for example, 1.5 g / 10 min, 3 g / 10 min, 5 g / 10 min, 8 g / 10 min, 9 g / 10 min), and a density of 0.88 to 0.98 g / cm 3 (For example, 0.89 g / cm 3 , 0.9g / cm 3 、0.94g / cm 3 , 0.96g / cm 3 ). In the present invention, the polyethylene may be one or more of low-density polyethylene, medium-density polyethylene and high-density polyethylene.
[0015] In one embodiment, the adhesive layer is a blend of POE-g-MAH and a tackifying resin; based on the total weight of the blend, the content of POE-g-MAH in the blend is 80wt% to 100wt% (e.g., 82wt%, 85wt%, 90wt%, 94wt%, 98wt%), and the content of the tackifying resin is 0wt% to 20wt% (e.g., 0.5wt%, 1wt%, 2wt%, 4wt%, 5wt%, 10wt%, 14wt%, 15wt%, 18wt%).
[0016] In one embodiment, the adhesive layer is a blend of POE-g-GMA and a tackifying resin; based on the total weight of the blend, the content of POE-g-GMA in the blend is 80wt% to 100wt% (e.g., 82wt%, 85wt%, 90wt%, 94wt%, 98wt%), and the content of the tackifying resin is 0wt% to 20wt% (e.g., 0.5wt%, 1wt%, 2wt%, 4wt%, 5wt%, 10wt%, 14wt%, 15wt%, 18wt%).
[0017] In one embodiment, the tackifying resin is a natural series resin and / or a synthetic series resin.
[0018] In one embodiment, the natural series resin is selected from one or more of rosin resin, rosin derivative resin and terpene resin (eg, α-terpene resin, β-terpene resin, terpene phenolic resin).
[0019] In one embodiment, the synthetic series resin is selected from polymer resins and / or condensation resins. Preferably, the polymer resin is selected from one or more of C5 petroleum resins, C9 petroleum resins, C5 / C9 petroleum resins, dicyclopentadiene (DCPD) resins, coumarone-indene resins and styrene series resins.
[0020] In one embodiment, the weight average molecular weight of the polyglycolic acid is 100,000 to 300,000 (for example, 120,000, 140,000, 150,000, 200,000, 250,000, or 280,000), and the melt index is 5.0 to 80 g / 10 min (for example, 6 g / 10 min, 10 g / 10 min, 15 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 60 g / 10 min, or 70 g / 10 min).
[0021] In one embodiment, the multi-layer high barrier film has a thickness of 50-300 μm (eg, 55 μm, 60 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm).
[0022] In one embodiment, the thickness ratio of each layer in the multi-layer high barrier film is outer layer: adhesive layer: barrier layer = 2:2:1 to 1:1:2, for example, 2:2:1.2, 2:2:1.4, 2:2:2, 2:2:2.4, 2:2:3, 2:2:3.6.
[0023] In a second aspect, a method for preparing the multilayer high barrier film as described above is provided, comprising the following steps:
[0024] (1) Weigh the raw material components for the outer layer, adhesive layer and barrier layer;
[0025] (2) In a multi-layer co-extruder, the raw material components of each layer are subjected to multi-layer co-extrusion, and the multi-layer high barrier film is obtained by a casting or blown film process;
[0026] In some embodiments, the interlayer adhesion of the multilayer high barrier film is greater than 2N / cm, for example, 2.1N / cm, 2.5N / cm, 4N / cm, 5N / cm, 8N / cm, 10N / cm; the water vapor transmission rate is ≤10g / (m 2 ·day), for example, 0.01g / (m 2 ·day)、0.05g / (m 2 ·day)、0.1g / (m 2 ·day)、0.5g / (m 2 ·day)、1.0g / (m 2 ·day)、2.0g / (m 2 ·day)、4.0g / (m2 ·day)、6.0g / (m 2 ·day)、8.0g / (m 2 ·day)、9.0g / (m 2 ·day); oxygen permeability ≤3cm 3 / (m 2 ·day·0.1MPa), for example, 0.01cm 3 / (m 2 ·day·0.1MPa)、0.05cm 3 / (m 2 ·day·0.1MPa)、0.1cm 3 / (m 2 ·day·0.1MPa)、0.5cm 3 / (m 2 ·day·0.1MPa)、1.0cm 3 / (m 2 ·day·0.1MPa)、2.0cm 3 / (m 2 ·day·0.1MPa)、2.5cm 3 / (m 2 ·day·0.1MPa).
[0027] According to the preparation method provided by the present invention, in some embodiments, in step (1), the raw material component of the adhesive layer is a blend of POE-g-MAH and a tackifying resin or a blend of POE-g-GMA and a tackifying resin; before multi-layer co-extrusion, POE-g-MAH and the tackifying resin or POE-g-GMA and the tackifying resin are weighed in proportion and blended, and melt-extruded and granulated by a twin-screw extruder to obtain a blend component as the adhesive layer.
[0028] In some embodiments, when preparing the blend, the process conditions of the melt extrusion include: the temperature of the conveying section of the extruder is 50-90°C (e.g., 60°C, 70°C), the temperature of the melting section is 120-150°C (e.g., 130°C, 140°C), the temperature of the mixing section is 130-160°C (e.g., 140°C, 150°C), the temperature of the exhaust section is 130-160°C (e.g., 140°C, 150°C), the temperature of the homogenizing section is 100-140°C (e.g., 120°C, 130°C); the screw speed is 50-200rpm (e.g., 60rpm, 100rpm, 150rpm).
[0029] In some embodiments, in step (2), the process conditions of the multi-layer co-extrusion include: the extrusion temperature of the outer layer is 140-220°C (e.g., 155°C, 170°C, 180°C, 200°C, 210°C); the extrusion temperature of the adhesive layer is 140-220°C (e.g., 155°C, 170°C, 180°C, 200°C, 210°C); the extrusion temperature of the barrier layer is 230-260°C (e.g., 235°C, 240°C, 245°C, 250°C); the die temperature is 240-260°C (e.g., 245°C, 250°C, 255°C).
[0030] In the preparation method of the present invention, the thickness of each layer in the multilayer film can be obtained by controlling the process parameters during extrusion.
[0031] In a third aspect, there is provided a multilayer film as described above or a multilayer film prepared by the preparation method as described above, for use in the packaging field, especially in food and drug packaging.
[0032] When pure PGA is used as a barrier layer in a multilayer film, there is often a problem of poor adhesion between pure PGA and other layer structures (such as PE), which is also the main technical obstacle to be solved by the patent of this invention.
[0033] In this field, the preparation of multilayer film can be carried out by hot pressing or multilayer coextrusion. Compared with the hot pressing of multilayer film, the multilayer coextrusion technology has the characteristics of continuous production and high efficiency. In the hot pressing process of multilayer film, each layer of structure is extruded separately and then molded. For the adhesive that plays a bonding role, oily and water-based adhesives can be selected, and the range of options is wide. For the multilayer coextrusion process, each layer must be directly coextruded to form a multilayer film using an extrusion process, so solution-type adhesives cannot be used, and the selection of materials used for the adhesive layer requires higher requirements.
[0034] The conventional adhesive layer in this field is maleic anhydride grafted polyethylene, but in the multilayer film co-extrusion process of this application, the applicant has found through research that when solving the existing technical obstacles, it is necessary to selectively select the adhesive layer material to ensure the improvement of the technical effect and meet the requirements.
[0035] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0036] The multilayer film prepared by the multilayer co-extrusion technology has the characteristics of continuous production and high efficiency; and in the multilayer co-extrusion process, the adhesive layer selected by the present application is conducive to further improving and increasing the bonding force between other layers and pure PGA. In addition, the barrier layer in the multilayer film of the present application is pure polyglycolic acid. On the basis of improving the bonding problem between polyethylene and polyglycolic acid, a non-stratified high barrier film can be prepared, and the multilayer film is degradable and has excellent water and oxygen barrier properties. DETAILED DESCRIPTION
[0037] In order to understand the technical features and contents of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described here.
[0038] <Source of raw materials>
[0039] Polyglycolic acid, weight average molecular weight of 130,000, melt index of 26 g / 10 min (240 ° C, 2.16 kg), purchased from Shanghai Pujing Chemical Technology Co., Ltd.;
[0040] Linear low-density polyethylene (LLDPE) 7042, density 0.92 g / cm 3 , melt flow rate (melt index) is 2.0 g / 10 min, purchased from Shenhua Baotou Chemical Co., Ltd.;
[0041] Tackifying resin, which is terpene resin, was purchased from Changzhou Jiatong Chemical Co., Ltd.;
[0042] POE-g-MAH, purchased from Dow Chemical;
[0043] POE-g-GMA was purchased from Jiayirong Co., Ltd.;
[0044] Silane coupling agent, purchased from Shandong Hengyu New Materials Co., Ltd.;
[0045] Other raw materials used in the examples and comparative examples are all commercially available conventional raw materials, which will not be described in detail here.
[0046] The structure of the multilayer film in each embodiment is schematically shown as: A / B / C / B / A, wherein A is the outer layer, B is the adhesive layer, and C is the barrier layer.
[0047] Embodiment 1:
[0048] A method for preparing a high barrier multilayer film comprises the following steps:
[0049] (1) Weighing raw material components such as polyethylene as an outer layer, POE-g-MAH as an adhesive layer, and polyglycolic acid as a barrier layer (inner layer);
[0050] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add POE-g-MAH to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 240-260°C and the roller temperature is 10-40°C; thereby obtaining a high barrier multilayer film.
[0051] The thickness of the multilayer film is 120 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0052] Embodiment 2:
[0053] A method for preparing a high barrier multilayer film comprises the following steps:
[0054] (1) Weighing raw material components such as polyethylene as an outer layer, POE-g-GMA as an adhesive layer, and polyglycolic acid as a barrier layer (inner layer);
[0055] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add POE-g-GMA to the core layer hopper, add polyethylene to the outer layer hopper, and extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner five layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 240-260°C and the roller temperature is 10-40°C; thus, a high barrier multilayer film is obtained.
[0056] The thickness of the multilayer film is 140 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0057] Embodiment 3:
[0058] A method for preparing a high barrier multilayer film comprises the following steps:
[0059] (1) Preparation of adhesive layer resin B1: 950 g of POE-g-MAH and 50 g of terpene resin were mixed and melt-extruded and granulated in a twin-screw extruder to obtain resin B1 as an adhesive layer; wherein the melt extrusion conditions are: the temperature of the conveying section is 70° C., the temperature of the melting section is 130° C., the temperature of the mixing section is 140° C., the temperature of the exhaust section is 140° C., the temperature of the homogenizing section is 120° C., and the screw speed is 100 rpm;
[0060] Weigh the raw material components such as polyethylene as the outer layer, resin B1 as the adhesive layer, and polyglycolic acid as the barrier layer (inner layer);
[0061] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add the prepared resin B1 to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 240-260°C and the roller temperature is 10-40°C; thereby obtaining a high barrier multilayer film.
[0062] The thickness of the multilayer film is 170 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0063] Embodiment 4:
[0064] A method for preparing a high barrier multilayer film comprises the following steps:
[0065] (1) Preparation of adhesive layer resin B2: 950 g of POE-g-GMA and 50 g of terpene resin were mixed and melt-extruded and granulated in a twin-screw extruder to obtain resin B2 as an adhesive layer; wherein the melt extrusion conditions are: the temperature of the conveying section is 70° C., the temperature of the melting section is 130° C., the temperature of the mixing section is 140° C., the temperature of the exhaust section is 140° C., the temperature of the homogenizing section is 120° C., and the screw speed is 100 rpm;
[0066] Weigh the raw material components such as polyethylene as the outer layer, resin B2 as the adhesive layer, and polyglycolic acid as the barrier layer (inner layer);
[0067] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add the prepared resin B2 to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast through a die to form a film, which is then rolled up. The die temperature is 240-260°C and the roller temperature is 10-40°C. A high barrier multilayer film is obtained.
[0068] The thickness of the multilayer film is 140 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0069] Embodiment 5:
[0070] The preparation method of the high barrier multilayer film is similar to that of Example 3, except that: in step (1), in the preparation of the adhesive layer resin B3, 900 g of POE-g-MAH and 100 g of terpene resin are mixed, melt-extruded, and granulated. The remaining steps are the same as those of Example 3.
[0071] The thickness of the multilayer film is 150 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0072] Embodiment 6:
[0073] The preparation method of the high barrier multilayer film is similar to that of Example 4, except that: in step (1), in the preparation of the adhesive layer resin B4, 850 g of POE-g-GMA and 150 g of terpene resin are melt-extruded and granulated in a twin-screw extruder. The remaining steps are the same as those of Example 4.
[0074] The thickness of the multilayer film is 150 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0075] Comparative Example 1:
[0076] The method for preparing a multilayer film comprises the following steps:
[0077] (1) Weighing raw material components such as polyethylene as an outer layer, polyethylene as an adhesive layer, and polyglycolic acid as a barrier layer (inner layer);
[0078] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add polyethylene to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 240-260°C and the roller temperature is 10-40°C.
[0079] The thickness of the prepared multilayer barrier film is 100 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0080] Comparative Example 2:
[0081] The method for preparing a multilayer film comprises the following steps:
[0082] (1) Weighing polyethylene raw materials for the inner layer, adhesive layer, and outer layer respectively;
[0083] (2) Polyethylene is added to the inner layer, core layer and outer layer hoppers of the co-extruder, and co-extruded through three screw extruders (the working temperatures of the inner layer, core layer and outer layer are 140-220°C, 140-220°C and 140-220°C respectively). The outer, middle and inner five layers are co-extruded and cast into a film through a die head, and then rolled up, wherein the die head temperature is 140-220°C and the roller temperature is 10-40°C.
[0084] The thickness of the prepared multilayer barrier film is 100 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0085] Comparative Example 3:
[0086] (1) Weighing raw material components such as polyethylene as an outer layer, PE-g-MAH as an adhesive layer, and polyglycolic acid as a barrier layer (inner layer);
[0087] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add PE-g-MAH to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, and then rolled up. The die head temperature is 240-260°C and the roller temperature is 10-40°C.
[0088] The thickness of the prepared multilayer barrier film is 150 μm; the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0089] Comparative Example 4:
[0090] The method for preparing a multilayer film comprises the following steps:
[0091] (1) Preparation of adhesive layer resin B5: 950 g of PE-g-MAH and 50 g of terpene resin were mixed and melt-extruded in a twin-screw extruder to obtain resin B5 as an adhesive layer; wherein the melt-extrusion conditions are: the temperature of the conveying section is 70° C., the temperature of the melting section is 130° C., the temperature of the mixing section is 140° C., the temperature of the exhaust section is 140° C., the temperature of the homogenizing section is 120° C., and the screw speed is 100 rpm;
[0092] Weigh the raw material components such as polyethylene as the outer layer, resin B5 as the adhesive layer, and polyglycolic acid as the barrier layer (inner layer);
[0093] (2) Add polyglycolic acid to the inner layer hopper of the co-extruder, add the prepared resin B5 to the core layer hopper, add polyethylene to the outer layer hopper, and co-extrude through three screw extruders (the working temperatures of the inner layer, core layer, and outer layer are 240-260°C, 140-220°C, and 140-220°C, respectively). The outer, middle, and inner layers are co-extruded and cast into a film through a die head, which is then rolled up. The die head temperature is 240-260°C and the roller temperature is 10-40°C.
[0094] The thickness of the prepared multilayer barrier film is 140 μm, and the thickness ratio of each layer is outer layer: adhesive layer: barrier layer = 1:1:1. The performance test of the film is shown in Table 1.
[0095] The test method is as follows:
[0096] (1) Melt index is measured according to the method described in GB / T 3682-2000;
[0097] (2) Water vapor transmission rate: measured according to the method described in GB / T 30412-2013;
[0098] (3) Oxygen transmission rate: measured according to the method described in GB / T 1038-2000;
[0099] (4) Peel strength test: measured according to GBT2792-2014 method.
[0100] Table 1 Performance test results of the multilayer films obtained in various embodiments and comparative examples
[0101]
[0102] Note: The “ / ” in Table 1 above means that the prepared film is delaminated and does not meet the requirements for the use of multilayer films, so there is no need to test the performance.
[0103] It can be seen from the experimental results in Table 1 that: by comparing Examples 1-6 with Comparative Example 2, the barrier properties of the multilayer film can be significantly improved by using composite PGA as a barrier layer; by comparing Examples 1-6 with Comparative Examples 1, 3, and 4, the adhesion problem between the layers in the multilayer barrier film can be effectively improved by preferably using a suitable component as an adhesive layer in the multilayer film. It can be seen from Examples 1-6 that adding a tackifying resin to the component used as the adhesive layer and changing the content of the tackifying resin can further improve the peel strength of the multilayer film.
[0104] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A multi-layer high barrier film, characterized in that: The multi-layer high barrier film comprises: an outer layer / adhesive layer / barrier layer / adhesive layer / outer layer arranged in sequence; wherein, The outer layer is polyethylene; The adhesive layer is selected from POE-g-MAH, POE-g-GMA, a blend of POE-g-MAH and a tackifying resin, and a blend of POE-g-GMA and a tackifying resin; The barrier layer is polyglycolic acid.
2. The multi-layer high barrier film according to claim 1, characterized in that: The polyethylene has a melt index of 1.0 to 10.0 g / 10 min and a density of 0.88 to 0.98 g / cm 3 .
3. The multi-layer high barrier film according to claim 1, characterized in that: The adhesive layer is a blend of POE-g-MAH and a tackifying resin; based on the total weight of the blend, the content of POE-g-MAH in the blend is 80wt% to 100wt%, and the content of the tackifying resin is 0wt% to 20wt%; or The adhesive layer is a blend of POE-g-GMA and a tackifying resin; based on the total weight of the blend, the content of POE-g-GMA in the blend is 80wt% to 100wt%, and the content of the tackifying resin is 0wt% to 20wt%.
4. The multi-layer high barrier film according to claim 1, characterized in that: The tackifying resin is a natural series resin and / or a synthetic series resin; Preferably, the natural series resin is selected from one or more of rosin resin, rosin derivative resin and terpene resin; Preferably, the synthetic series resin is selected from polymer resins and / or condensation resins; more preferably, the polymer resin is selected from one or more of C5 petroleum resin, C9 petroleum resin, C5 / C9 petroleum resin, dicyclopentadiene resin, coumarone-indene resin and styrene series resins.
5. The multi-layer high barrier film according to claim 1, characterized in that: The weight average molecular weight of the polyglycolic acid is 100,000 to 300,000, and the melt index is 5.0 to 80 g / 10 min.
6. The multi-layer high barrier film according to claim 1, characterized in that: The thickness of the multilayer high barrier film is 50-300 μm; The thickness ratio of each layer in the multi-layer high barrier film is outer layer: adhesive layer: barrier layer = 2:2:1 to 1:1:
2.
7. The method for preparing a multilayer high barrier film according to any one of claims 1 to 6, characterized in that: The steps include: (1) Weigh the raw material components for the outer layer, adhesive layer and barrier layer; (2) In a multi-layer co-extruder, the raw material components of each layer are subjected to multi-layer co-extrusion, and the multi-layer high barrier film is obtained by a casting or blown film process; Preferably, the interlayer adhesion of the multilayer high barrier film is greater than 2N / cm; the water vapor transmission rate is ≤10g / (m 2 ·day); oxygen permeability ≤3cm 3 / (m 2 ·day·0.1MPa).
8. The preparation method according to claim 7, characterized in that: In step (1), the raw material component of the adhesive layer is a blend of POE-g-MAH and a tackifying resin or a blend of POE-g-GMA and a tackifying resin; before multi-layer co-extrusion, POE-g-MAH and the tackifying resin or POE-g-GMA and the tackifying resin are weighed and blended according to a proportion, and melt-extruded and granulated by a twin-screw extruder to obtain a blend component as the adhesive layer; Preferably, the process conditions of melt extrusion include: the temperature of the conveying section of the extruder is 50-90°C, the temperature of the melting section is 120-150°C, the temperature of the mixing section is 130-160°C, the temperature of the exhaust section is 130-160°C, the temperature of the homogenizing section is 100-140°C; the screw speed is 50-200rpm.
9. The preparation method according to claim 7, characterized in that: In step (2), the process conditions of the multi-layer co-extrusion include: the extrusion temperature of the outer layer is 140-220°C; the extrusion temperature of the adhesive layer is 140-220°C; the extrusion temperature of the barrier layer is 230-260°C; and the die head temperature is 240-260°C.
10. Use of the multilayer film according to any one of claims 1 to 6 or the multilayer film prepared by the preparation method according to any one of claims 7 to 9 in the packaging field, especially in food and drug packaging.
Citation Information
Patent Citations
Multilayer tube for transporting water or gas
CN101326055A
Composite film with gas barrier property
JP1998080990A
Resin laminate and stretched film using the same
JP2008132687A
Multilayered stretched film and packaging material obtained by using the same
JP2013141784A