Polycarbonate diol composition and preparation method thereof
Through the composition of polycarbonate diol, secondary modified polycarbonate polyol and small molecule diesters, ether bonds and ester bonds are introduced, the traditional polycarbonate diol is solved in high temperature and high humidity environment. Performance stability issues improve weather resistance, oxidation resistance and ultraviolet resistance, and are suitable for many industrial fields.
Patent Information
- Application Number
- CN202411378916.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polycarbonate diols have poor performance stability in high temperature and high humidity environments, and their weather resistance, oxidation resistance and ultraviolet resistance are insufficient, so they cannot maintain stable comprehensive and mechanical properties under various environmental conditions.
Using a composition of polycarbonate diol, a secondary modified polycarbonate polyol and a small molecule diester, a bio-based 1,3-propylene glycol, 1,4-butanediol, dimethyl carbonate, dicarbonate The reaction preparation of phenyl ester is introduced, ether bonds and ester bonds are introduced, and isopropyl titanate is used as a catalyst to perform multi-step modification treatment to improve material performance.
The weather resistance, oxidation resistance and ultraviolet resistance of the polycarbonate diol composition are significantly improved, so that the prepared polymer materials maintain stable comprehensive and mechanical properties under various environmental conditions, extending their service life, and Suitable for many fields such as coatings, elastomers and plastics.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of polycarbonate diols, in particular to a polycarbonate diol composition and a preparation method thereof. Background Art
[0002] Polyurethane resins are widely used in synthetic leather, artificial leather, adhesives, furniture coatings, automotive coatings and other fields. As one of the raw materials of polyurethane resins, polyol components mainly include polyether, polyester and polycarbonate. Among them, polyether polyols have low viscosity, which makes the polyurethane prepared by polyether polyols excellent in softness and hydrolysis resistance, but poor in heat resistance and weather resistance. Polyester polyols can improve the heat resistance and weather resistance of polyurethane, but poor in hydrolysis resistance. Polycarbonate polyols show the best durability level in terms of heat resistance, chemical resistance and hydrolysis resistance. The polycarbonate polyurethane resin prepared by polycarbonate polyols, in addition to the advantages of polyether and polyester polyurethanes, also has good wear resistance, weather resistance, oil resistance and mildew resistance, and is widely used in the fields of shoemaking, plastic tracks and building sealing. In addition, due to its good biocompatibility, it can also be used as medical devices and artificial organs in the medical and health fields.
[0003] As an important polymer compound, polycarbonate diol is widely used in the fields of polyurethane, polycarbonate resin, etc. due to its unique chemical structure and properties. However, the performance stability of polyurethane, polycarbonate resin and other polymer materials prepared using traditional polycarbonate diol as raw material is not ideal under certain specific application conditions (such as high temperature, high humidity and other environments), and it is impossible to maintain stable comprehensive performance and mechanical properties under various environmental conditions, and the weather resistance needs to be further improved; at the same time, in order to further expand the application scope of the above-mentioned polymer materials, their antioxidant and UV resistance properties also need to be further improved.
[0004] Therefore, a novel polycarbonate diol composition and a preparation method thereof are provided. Polyurethane, polycarbonate resin and other polymer materials prepared using the polycarbonate diol composition can maintain stable comprehensive performance and mechanical properties under various environmental conditions while further improving the weather resistance, oxidation resistance, UV resistance and overall stability of the aforementioned polymer materials, which has important practical application value and technical significance. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the present invention provides a polycarbonate diol composition and a preparation method thereof. Polyurethane, polycarbonate resin and other polymer materials prepared using the polycarbonate diol composition can maintain stable comprehensive performance and mechanical properties under various environmental conditions while further improving the weather resistance, antioxidant performance, UV resistance and overall stability of the aforementioned polymer materials.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A polycarbonate diol composition is prepared from the following raw materials: 60-90 parts of polycarbonate diol, 10-30 parts of secondary modified polycarbonate polyol, 0.1-5 parts of small molecule dibasic ester, and 0.1-5 parts of catalyst; The polycarbonate diol is prepared by reacting bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate and diphenyl carbonate as raw materials; The secondary modified polycarbonate polyol is a modified polycarbonate polyol with ether bonds and ester bonds introduced; The small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; The catalyst is isopropyl titanate.
[0007] Preferably, the polycarbonate diol comprises 80-90 parts, the secondary modified polycarbonate polyol comprises 18-22 parts, the small molecule dibasic ester comprises 3-3.5 parts, and the catalyst comprises 0.3-0.4 parts.
[0008] A method for preparing a polycarbonate diol composition comprises the following steps: preparing polycarbonate diol, preparing a primary modified polycarbonate polyol, preparing a secondary modified polycarbonate polyol, and preparing a composition.
[0009] The method for preparing polycarbonate diol comprises the following steps: adding bio-based 1,3-propylene glycol, bio-based 1,4-butanediol and catalyst dibutyltin dilaurate into a reaction kettle, heating the mixture to 150-160° C., stirring the mixture while keeping the temperature constant, and simultaneously dripping dimethyl carbonate and diphenyl carbonate into the reaction kettle; after the dripping is completed, continuing to keep the temperature constant and stirring the mixture, and then evaporating and removing unreacted excess raw materials and by-product impurities, adjusting the vacuum degree of the reaction kettle to 700-800 Pa, continuing to heat the mixture to 185-190° C., and carrying out a reaction while keeping the temperature constant to obtain polycarbonate diol.
[0010] In the preparation of the polycarbonate diol, the molar ratio of bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate, and diphenyl carbonate is 0.4-0.6:0.4-0.6:0.42-0.62:0.42-0.62; The added amount of the catalyst dibutyltin dilaurate is 0.25-0.3% of the weight of dimethyl carbonate.
[0011] The structural formula of the polycarbonate diol is as follows:
[0012] Wherein, R1, R2, and R3 are different hydrocarbon groups; the hydrocarbon group is preferably one of the following: propyl, butyl, and phenyl.
[0013] The method for preparing a primary modified polycarbonate polyol comprises the following steps: adding polypropylene glycol PPG-400, propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and a catalyst zinc-cobalt double metal cyanide into a clean, water-free autoclave, sealing the autoclave, introducing carbon dioxide into the autoclave until the pressure in the autoclave reaches 3.5-4 MPa, heating the autoclave to 75-80° C., keeping the temperature for reaction for 8-10 hours, naturally cooling the autoclave to room temperature, depressurizing the autoclave to normal pressure, evaporating and removing excess propylene oxide, and obtaining the primary modified polycarbonate polyol; In the preparation of the once-modified polycarbonate polyol, the weight ratio of polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and catalyst zinc-cobalt double metal cyanide is 20-24:70-80:16-16.5:3-3.3:0.12-0.16.
[0014] The method for preparing the secondary modified polycarbonate polyol comprises the following steps: adding the primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine into a reaction kettle containing dichloromethane, stirring for 20-30 minutes, heating to 32-36°C, and reacting by keeping the temperature and stirring for 22-24 hours to obtain a reaction liquid; using n-hexane 4-5 times the volume of the reaction liquid for precipitation, filtering out solids; washing the solids with deionized water 1.5-2 times the volume, and evaporating to remove the solvent to obtain the secondary modified polycarbonate polyol.
[0015] In the preparation of the secondary modified polycarbonate polyol, the molar ratio of the primary modified polycarbonate polyol, hydroxyethyl methacrylate, and catalyst pyridine is 1:2-2.1:0.8-0.85; The weight ratio of the primary modified polycarbonate polyol to dichloromethane is 1:1.4-1.5.
[0016] The method for preparing the composition comprises: uniformly mixing polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst isopropyl titanate, carrying out heat preservation polymerization reaction for 16-18 hours at a temperature of 140-150° C. and a pressure of 0.5-0.6 MPa, and then cooling and solidifying to obtain a polycarbonate diol composition; In the prepared composition, the small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate.
[0017] In the composition, the weight ratio of polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst is 60-90:10-30:0.1-5:0.1-5; preferably, the weight ratio of polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst isopropyl titanate is 80-90:18-22:3-3.5:0.3-0.4; The weight ratio of dimethyl carbonate to ethylene carbonate is 2.2-2.5:1.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) The preparation method of the polycarbonate diol composition of the present invention comprises the following steps: polycarbonate diol is prepared by combining with a secondary modified polycarbonate polyol and a small molecule dibasic ester; and in the step of preparing the polycarbonate diol, bio-based 1,3-propylene glycol and bio-based 1,4-butanediol are combined with dimethyl carbonate and diphenyl carbonate to prepare the polycarbonate diol, so as to obtain a polycarbonate diol containing propyl, butyl and phenyl groups; and then in the step of preparing the primary modified polycarbonate polyol, 3-isocyanate propyl triethoxysilane and isopropyl trioleyl titanate are combined to modify the polyether / polycarbonate polyol, so as to improve the synthesis efficiency and catalyze the reaction process, and further improve the resistance of the polycarbonate diol composition. The invention discloses a method for preparing a secondary modified polycarbonate polyol, wherein the polycarbonate polyol is prepared by using an ester bond-capping agent, hydroxyethyl methacrylate, for further modification, and further introducing ester bonds into the polycarbonate polyol to obtain a secondary modified polycarbonate polyol; the performance stability of the polycarbonate diol composition is further improved by introducing ether bonds and ester bonds into the modified polycarbonate polyol, so that the polyurethane, polycarbonate resin and other polymer materials prepared by using the polycarbonate diol composition can maintain stable comprehensive performance and mechanical properties under various environmental conditions, while further improving the weather resistance, oxidation resistance, UV resistance and overall stability of the aforementioned polymer materials.
[0020] 2) The polycarbonate diol composition of the present invention has good performance stability. When the polyurethane, polycarbonate resin and other polymer materials prepared by using the composition are used, the mechanical properties and weather resistance of the polyurethane, polycarbonate resin and other polymer materials can be effectively improved, and the overall stability is good.
[0021] 3) The polycarbonate diol composition of the present invention has excellent weather resistance and overall stability, can maintain stable comprehensive performance and mechanical properties under various environmental conditions, and effectively prolong the service life of the corresponding products; at the same time, the polycarbonate diol composition has good antioxidant and UV resistance, further improving the durability and stability of its corresponding products; it can be widely used in the fields of plastics, coatings, elastomers, etc., providing excellent performance and functions. For example, in the field of coatings, it can increase the softness, adhesion, water resistance and chemical resistance of coatings; in the field of elastomers, it can be used to manufacture various sealing, shock absorption, vibration prevention, noise reduction and buffering materials; in the field of plastics, it can manufacture plastic products with high strength, high transparency and high glass transition temperature.
[0022] 4) The preparation method of the polycarbonate diol composition of the present invention is simple, the process is easy to control, and it is suitable for industrial production; at the same time, the polycarbonate diol composition has good processing performance. When it is used to prepare polymer materials, it has little effect on the stability of the polymer material formula, which is beneficial to the production and processing of the corresponding polymer materials.
[0023] 5) The polycarbonate diol composition of the present invention has good performance adjustability. By changing and adjusting the ratio of raw materials such as polycarbonate diol and secondary modified polycarbonate polyol, corresponding polymer materials that meet the requirements of different fields can be prepared, thereby meeting the application requirements of different fields and having good applicability. DETAILED DESCRIPTION
[0024] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described. Example 1
[0025] This embodiment provides a method for preparing a polycarbonate diol composition, which is prepared using the following raw materials: 80 parts of polycarbonate diol, 18 parts of secondary modified polycarbonate polyol, 3 parts of small molecule dibasic ester, and 0.3 parts of catalyst; The small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; the weight ratio of dimethyl carbonate to ethylene carbonate is 2.2:1.
[0026] The catalyst is isopropyl titanate.
[0027] The method for preparing the polycarbonate diol composition comprises the following steps: preparing polycarbonate diol, preparing primary modified polycarbonate polyol, preparing secondary modified polycarbonate polyol and preparing the composition.
[0028] The specific steps are as follows: 1. Preparation of polycarbonate diol Bio-based 1,3-propylene glycol, bio-based 1,4-butanediol and catalyst dibutyltin dilaurate are put into a reactor, heated to 150°C, stirred and kept warm, and dimethyl carbonate and diphenyl carbonate are added dropwise at the same time; the addition time of dimethyl carbonate and diphenyl carbonate is controlled to be 8 hours. After the addition is completed, the stirring is continued for 4 hours, and after evaporating to remove the unreacted excess raw materials and by-product impurities, the vacuum degree of the reactor is adjusted to 700Pa, and the temperature is continued to be raised to 185°C. After the reaction is kept warm for 3 hours, polycarbonate diol is obtained.
[0029] The molar ratio of bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate, and diphenyl carbonate is 0.4:0.4:0.42:0.42; The amount of catalyst dibutyltin dilaurate added is 0.25% by weight of dimethyl carbonate.
[0030] 2. Preparation of primary modified polycarbonate polyol Put polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate and catalyst zinc-cobalt double metal cyanide into a clean, water-free autoclave, seal the autoclave, introduce carbon dioxide into the autoclave until the pressure in the autoclave reaches 3.5 MPa, heat to 75°C, keep the temperature for reaction for 8 hours, cool naturally to room temperature, release the pressure of the autoclave to normal pressure, evaporate and remove excess propylene oxide, and obtain a primary modified polycarbonate polyol.
[0031] Among them, the weight ratio of polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and catalyst zinc-cobalt double metal cyanide is 20:70:16:3:0.12.
[0032] 3. Preparation of secondary modified polycarbonate polyol The primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine are put into a reactor containing dichloromethane, stirred for 20 minutes, heated to 32°C, and stirred for 22 hours to obtain a reaction liquid; 4 times the volume of n-hexane of the reaction liquid is used for precipitation, and the solid is filtered out; the solid is washed with 1.5 times the volume of deionized water, and the solvent is evaporated to obtain a secondary modified polycarbonate polyol.
[0033] The molar ratio of the primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine is 1:2:0.8.
[0034] The weight ratio of the primary modified polycarbonate polyol to dichloromethane is 1:1.4.
[0035] 4. Preparation of composition According to the above-mentioned weight parts, polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst isopropyl titanate were uniformly mixed, and then the mixture was kept warm and polymerized for 16 hours at a temperature of 140° C. and a pressure of 0.5 MPa, and then cooled and solidified to obtain a polycarbonate diol composition.
[0036] This embodiment also provides a polycarbonate diol composition prepared by the above-mentioned preparation method.
[0037] Example 2 This embodiment provides a method for preparing a polycarbonate diol composition, which is prepared using the following raw materials: 85 parts of polycarbonate diol, 20 parts of secondary modified polycarbonate polyol, 3.2 parts of small molecule dibasic ester, and 0.35 parts of catalyst; The small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; the weight ratio of dimethyl carbonate to ethylene carbonate is 2.3:1.
[0038] The catalyst is isopropyl titanate.
[0039] The method for preparing the polycarbonate diol composition comprises the following steps: preparing polycarbonate diol, preparing primary modified polycarbonate polyol, preparing secondary modified polycarbonate polyol and preparing the composition.
[0040] The specific steps are as follows: 1. Preparation of polycarbonate diol Bio-based 1,3-propylene glycol, bio-based 1,4-butanediol and catalyst dibutyltin dilaurate were put into a reactor, heated to 155°C, stirred while keeping warm, and dimethyl carbonate and diphenyl carbonate were added dropwise at the same time; the addition time of dimethyl carbonate and diphenyl carbonate was controlled to be 8.5h. After the addition was completed, the stirring was continued for 4.5h, and the unreacted excess raw materials and by-product impurities were evaporated to remove the unreacted excess raw materials and by-product impurities, and the vacuum degree of the reactor was adjusted to 750Pa, and the temperature was continued to be raised to 187°C. After the reaction was kept warm for 3.5h, polycarbonate diol was obtained.
[0041] Among them, the molar ratio of bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate and diphenyl carbonate is 0.5:0.5:0.52:0.52.
[0042] The added amount of the catalyst dibutyltin dilaurate is 0.28% of the weight of dimethyl carbonate.
[0043] 2. Preparation of primary modified polycarbonate polyol Put polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate and catalyst zinc-cobalt double metal cyanide into a clean, water-free autoclave, seal the autoclave, introduce carbon dioxide into the autoclave until the pressure in the autoclave reaches 3.8 MPa, heat to 78°C, keep the reaction for 9 hours, cool naturally to room temperature, release the pressure of the autoclave to normal pressure, evaporate and remove excess propylene oxide, and obtain a primary modified polycarbonate polyol.
[0044] Among them, the weight ratio of polypropylene glycol (PPG-400), propylene oxide, 3-isocyanatepropyltriethoxysilane, isopropyltrioleate acyloxytitanate, and catalyst zinc-cobalt double metal cyanide is 22:75:16.3:3.2:0.15.
[0045] 3. Preparation of secondary modified polycarbonate polyol The primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine were put into a reactor filled with dichloromethane, stirred for 25 minutes, heated to 35°C, and stirred for 23 hours to obtain a reaction liquid; 4.5 times the volume of n-hexane of the reaction liquid was used for precipitation, and the solid was filtered out; the solid was washed with 1.8 times the volume of deionized water, and the solvent was evaporated to obtain a secondary modified polycarbonate polyol.
[0046] The molar ratio of the primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine is 1:2.05:0.83.
[0047] The weight ratio of the primary modified polycarbonate polyol to dichloromethane is 1:1.45.
[0048] 4. Preparation of composition According to the above-mentioned weight parts, polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst isopropyl titanate were uniformly mixed, and then the mixture was kept warm and polymerized for 17 hours at a temperature of 145° C. and a pressure of 0.55 MPa, and then cooled and solidified to obtain a polycarbonate diol composition.
[0049] This embodiment also provides a polycarbonate diol composition prepared by the above-mentioned preparation method.
[0050] Example 3 This embodiment provides a method for preparing a polycarbonate diol composition, which is prepared using the following raw materials: 80-90 parts of polycarbonate diol, 22 parts of secondary modified polycarbonate polyol, 3.5 parts of small molecule dibasic ester, and 0.4 parts of catalyst; The small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; the weight ratio of dimethyl carbonate to ethylene carbonate is 2.5:1.
[0051] The catalyst is isopropyl titanate.
[0052] The method for preparing the polycarbonate diol composition comprises the following steps: preparing polycarbonate diol, preparing primary modified polycarbonate polyol, preparing secondary modified polycarbonate polyol and preparing the composition.
[0053] The specific steps are as follows: 1. Preparation of polycarbonate diol Bio-based 1,3-propylene glycol, bio-based 1,4-butanediol and catalyst dibutyltin dilaurate are put into a reactor, heated to 160°C, stirred and kept warm, and dimethyl carbonate and diphenyl carbonate are added dropwise at the same time; the addition time of dimethyl carbonate and diphenyl carbonate is controlled to be 9 hours. After the addition is completed, the mixture is kept warm and stirred for 5 hours. After evaporating to remove the unreacted excess raw materials and by-product impurities, the vacuum degree of the reactor is adjusted to 800 Pa, and the temperature is continued to be raised to 190°C. After the reaction is kept warm for 4 hours, polycarbonate diol is obtained.
[0054] Among them, the molar ratio of bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate and diphenyl carbonate is 0.6:0.6:0.62:0.62.
[0055] The added amount of the catalyst dibutyltin dilaurate is 0.3% of the weight of dimethyl carbonate.
[0056] 2. Preparation of primary modified polycarbonate polyol Put polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate and catalyst zinc-cobalt double metal cyanide into a clean, water-free autoclave, seal the autoclave, introduce carbon dioxide into the autoclave until the pressure in the autoclave reaches 4 MPa, heat to 80°C, keep the temperature for reaction for 10 hours, cool naturally to room temperature, release the pressure of the autoclave to normal pressure, evaporate and remove excess propylene oxide, and obtain a primary modified polycarbonate polyol.
[0057] Among them, the weight ratio of polypropylene glycol (PPG-400), propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and catalyst zinc-cobalt double metal cyanide is 24:80:16.5:3.3:0.16.
[0058] 3. Preparation of secondary modified polycarbonate polyol The primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine are put into a reactor containing dichloromethane, stirred for 30 minutes, heated to 36°C, kept stirred and reacted for 24 hours to obtain a reaction liquid; 5 times the volume of n-hexane of the reaction liquid is used for precipitation, and the solid is filtered out; the solid is washed with 2 times the volume of deionized water, and the solvent is evaporated to obtain a secondary modified polycarbonate polyol.
[0059] The molar ratio of the primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine is 1:2.1:0.85.
[0060] The weight ratio of the primary modified polycarbonate polyol to dichloromethane is 1:1.5.
[0061] 4. Preparation of composition According to the above-mentioned weight parts, polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst isopropyl titanate were uniformly mixed, and then the mixture was kept warm and polymerized for 18 hours at a temperature of 150° C. and a pressure of 0.6 MPa, and then cooled and solidified to obtain a polycarbonate diol composition.
[0062] This embodiment also provides a polycarbonate diol composition prepared by the above-mentioned preparation method.
[0063] Comparative Example 1 The method for preparing the polycarbonate diol of Example 2 is adopted, but the differences are that 1) in the step of preparing the primary modified polycarbonate polyol, the use of 3-isocyanatepropyltriethoxysilane and isopropyltrioleyltitanate is omitted; 2) the step of preparing the secondary modified polycarbonate polyol is omitted, and the polycarbonate polyol prepared in the previous step (the step of preparing the primary modified polycarbonate polyol) is used in the subsequent step.
[0064] The polycarbonate diol compositions of Examples 1-3 and Comparative Example 1 were respectively used in the preparation of polyurethane. Specifically, the polycarbonate diol composition and N,N-dimethylformamide were respectively added into a reactor, stirred and heated to 60°C. After being kept warm and stirred for 40 minutes, 1,4-butanediol and dibutyltin dilaurate were added, and then diphenylmethane diisocyanate melt was dripped in, and the dripping rate of the diphenylmethane diisocyanate melt was controlled to be 1.2 g / min. After the dripping was completed, the reaction was kept warm and stirred until the weight average molecular weight was not less than 100,000. After terminating the reaction, the solid content was adjusted to 30wt% to obtain an N,N-dimethylformamide solution of polyurethane.
[0065] The weight ratio of the polycarbonate diol composition, N,N-dimethylformamide, 1,4-butanediol, dibutyltin dilaurate and diphenylmethane diisocyanate is 205:770:9:0.06:51.
[0066] Then, the polyurethane N,N-dimethylformamide solution was evenly coated on the surface of the substrate by a doctor blade coating method, and then dried to obtain a polyurethane film; and the thickness of the polyurethane films obtained from the polycarbonate diol compositions of Control Examples 1-3 and Comparative Example 1 was the same. The tensile strength and elongation at break of each polyurethane film were tested respectively.
[0067] At the same time, the following tests were carried out on each polyurethane film: In the heat aging test, each polyurethane film was placed at 80°C for 30 days, and then the tensile strength retention rate and the elongation at break retention rate were detected and calculated.
[0068] In the hydrolysis stability test, each polyurethane film was completely immersed in water at 70° C. and allowed to stand for 30 days. Then, the tensile strength retention rate and the elongation at break retention rate were detected and calculated.
[0069] In the UV resistance test, each polyurethane film was placed in a UV aging tester and continuously exposed to accelerated UVB for 1500 hours. The gloss retention rate of each polyurethane film was then detected and calculated. After the exposure, it was observed whether the polyurethane film had any cracks or powdering.
[0070] In the stability test, each polyurethane film was placed in an environment with a temperature of 45°C and a relative humidity of 85%. After continuous irradiation with an 800W xenon lamp for 1000 hours, the tensile strength retention rate and the elongation at break retention rate were detected and calculated.
[0071] The specific results are shown in the following table:
[0072] It can be seen that the preparation method of the polycarbonate diol composition of the present invention adopts polycarbonate diol and secondary modified polycarbonate polyol and small molecule dibasic ester to prepare polycarbonate diol by using bio-based 1,3-propylene glycol and bio-based 1,4-butanediol in combination with dimethyl carbonate and diphenyl carbonate in the step of preparing polycarbonate diol to obtain polycarbonate diol containing propyl, butyl and phenyl groups; and then in the step of preparing primary modified polycarbonate polyol, 3-isocyanate propyl triethoxysilane and isopropyl trioleyl titanate are used to modify polyether / polycarbonate polyol, so as to improve the synthesis efficiency, catalyze the reaction process, and further improve the polycarbonate diol composition. Weather resistance and overall stability are improved, and mechanical properties are optimized; then in the step of preparing the secondary modified polycarbonate polyol, hydroxyethyl methacrylate containing an ester bond capping agent is used for further modification treatment, and ester bonds are further introduced into the polycarbonate polyol to obtain the secondary modified polycarbonate polyol; the performance stability of the polycarbonate diol composition is further improved by introducing ether bonds and ester bonds into the modified polycarbonate polyol, so that the polyurethane, polycarbonate resin and other polymer materials prepared by the polycarbonate diol composition can maintain stable comprehensive performance and mechanical properties under various environmental conditions, while further improving the weather resistance, antioxidant performance, UV resistance and overall stability of the aforementioned polymer materials.
[0073] Unless otherwise specified, all percentages used in the present invention are by mass.
[0074] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A polycarbonate diol composition, characterized in that: The following raw materials are used to prepare the method: 60-90 parts of polycarbonate diol, 10-30 parts of secondary modified polycarbonate polyol, 0.1-5 parts of small molecule dibasic ester, and 0.1-5 parts of catalyst; The polycarbonate diol is prepared by reacting bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate and diphenyl carbonate as raw materials; The secondary modified polycarbonate polyol is a modified polycarbonate polyol with ether bonds and ester bonds introduced; The small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; The catalyst is isopropyl titanate.
2. A method for preparing a polycarbonate diol composition, characterized in that: The method comprises the following steps: preparing polycarbonate diol, preparing primary modified polycarbonate polyol, preparing secondary modified polycarbonate polyol and preparing a composite; The method for preparing polycarbonate diol comprises: adding bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, and a catalyst dibutyltin dilaurate into a reaction kettle, heating the mixture to 150-160° C., stirring the mixture while keeping the temperature high, and simultaneously dripping dimethyl carbonate and diphenyl carbonate; after the dripping is completed, continuing to keep the temperature high and stirring the mixture, and then evaporating and removing the unreacted excess raw materials and by-product impurities, adjusting the vacuum degree of the reaction kettle to 700-800 Pa, and continuing to heat the mixture to 185-190° C., and reacting the mixture while keeping the temperature high to obtain polycarbonate diol; The method for preparing a primary modified polycarbonate polyol comprises the following steps: adding polypropylene glycol PPG-400, propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and a catalyst zinc-cobalt double metal cyanide into a clean, water-free autoclave, sealing the autoclave, introducing carbon dioxide into the autoclave until the pressure in the autoclave reaches 3.5-4 MPa, heating the autoclave to 75-80° C., keeping the temperature for reaction, naturally cooling to room temperature, depressurizing the autoclave to normal pressure, evaporating and removing excess propylene oxide, and obtaining the primary modified polycarbonate polyol; The method for preparing the secondary modified polycarbonate polyol comprises: adding the primary modified polycarbonate polyol, hydroxyethyl methacrylate and catalyst pyridine into dichloromethane, mixing them evenly, heating them to 32-36° C., stirring and reacting them at the temperature, and obtaining a reaction liquid; using n-hexane for precipitation, filtering out solids; washing the solids, removing the solvent, and obtaining the secondary modified polycarbonate polyol; The method for preparing the composition comprises: uniformly mixing polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst, carrying out heat preservation polymerization reaction at a temperature of 140-150° C. and a pressure of 0.5-0.6 MPa, cooling and solidifying to obtain a polycarbonate diol composition; In the preparation composition, the small molecule dibasic ester is a mixture of dimethyl carbonate and ethylene carbonate; In the preparation composition, the catalyst is isopropyl titanate.
3. The method for preparing the polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the polycarbonate diol, the dropwise addition time of dimethyl carbonate and diphenyl carbonate is 8-9 hours; The heat preservation and stirring time after the addition of dimethyl carbonate and diphenyl carbonate is completed is 4-5 hours; The heat preservation reaction time at 185-190°C is 3-4h.
4. The method for preparing the polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the polycarbonate diol, the molar ratio of bio-based 1,3-propylene glycol, bio-based 1,4-butanediol, dimethyl carbonate, and diphenyl carbonate is 0.4-0.6:0.4-0.6:0.42-0.62:0.42-0.62; The added amount of the catalyst dibutyltin dilaurate is 0.25-0.3% of the weight of dimethyl carbonate.
5. The method for preparing the polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the primary modified polycarbonate polyol, the heat preservation reaction time at a temperature of 75-80° C. is 8-10 hours.
6. The method for preparing the polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the once-modified polycarbonate polyol, the weight ratio of polypropylene glycol PPG-400, propylene oxide, 3-isocyanate propyl triethoxysilane, isopropyl trioleate acyloxy titanate, and catalyst zinc-cobalt double metal cyanide is 20-24:70-80:16-16.5:3-3.3:0.12-0.
16.
7. The method for preparing a polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the secondary modified polycarbonate polyol, the heat preservation reaction time at a temperature of 32-36° C. is 22-24 hours.
8. The method for preparing the polycarbonate diol composition according to claim 2, characterized in that: In the preparation of the secondary modified polycarbonate polyol, the molar ratio of the primary modified polycarbonate polyol, hydroxyethyl methacrylate, and catalyst pyridine is 1:2-2.1:0.8-0.85; The weight ratio of the primary modified polycarbonate polyol to dichloromethane is 1:1.4-1.
5.
9. The method for preparing a polycarbonate diol composition according to claim 2, characterized in that: In the composition, the weight ratio of polycarbonate diol, secondary modified polycarbonate polyol, small molecule dibasic ester and catalyst is 60-90:10-30:0.1-5:0.1-5; The heat preservation polymerization reaction time is 16-18h; The weight ratio of dimethyl carbonate to ethylene carbonate is 2.2-2.5:1.
Citation Information
Patent Citations
Polymer compositions and methods
CN103827207A
Method for producing polycarbonate diol and polycarbonate diol, and method for producing polyurethane and polyurethane
CN105452332A
White polycarbonate composition with high toughness and high glow wire initiation temperature and preparation method thereof
CN106916429A
Polycarbonate polyol and polyurethane
CN110099943A