Polyelectrolyte hybridized polydopamine nano-particles as well as preparation method and application thereof

Through the hybridization reaction of polyethyleneimine and dopamine hydrochloride, polyelectrolyte hybrid polydopamine nanoparticles with high lipophilic anion graft density were prepared, which solved the dispersion stability of polydopamine nanoparticles in oil and significantly improved the The wear resistance of lubricating oil.

CN118895046APending Publication Date: 2024-11-05CHENGDU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410944265.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The poor dispersion stability of polydopamine nanoparticles in oil limits their application as a friction-reducing and anti-wear additive for lubricating oil.

Method used

Using the hybridization reaction of polyethyleneimine and dopamine hydrochloride, polyelectrolyte hybrid polydopamine nanoparticles with high lipophilic anionic graft density are prepared to improve their dispersion in oil. Stability and lubricating properties.

Benefits of technology

The stable dispersion and lubrication performance of polydopamine nanoparticles in oil are achieved, which significantly improves the wear resistance of lubricating oil, and simplifies the preparation process, avoiding the harsh condition control in the two-step grafting method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895046A_ABST
    Figure CN118895046A_ABST
Patent Text Reader

Abstract

The invention discloses a polyelectrolyte hybrid polydopamine nanoparticle as well as a preparation method and application thereof, and belongs to the technical field of material preparation. A catechol group of polydopamine and an amino group of PEI are subjected to a Michael addition reaction, polyethyleneimine modified polydopamine nanoparticles are obtained through a one-pot method, and the dispersing capacity of the polydopamine nanoparticles in base oil is improved through modification. According to the invention, polyethyleneimine with different molecular weights is utilized to provide an alkaline environment required by polymerization of dopamine hydrochloride, and serves as a surface modifier, so that the surfaces of synthesized polydopamine nanoparticles have sufficient active amino groups, thereby effectively improving the binding rate of oil-soluble anions, and improving the polymerization efficiency of the oil-soluble anions. The polydopamine nanoparticles are dispersed in the base oil permanently and stably, the obtained polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs) can be directly dispersed in the polyethylene glycol base oil, and the antifriction and antiwear properties of the base oil are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a polyelectrolyte hybrid polydopamine nanoparticle and a preparation method and application thereof. Background Art

[0002] Polydopamine nanoparticles are a kind of polymer nanomaterial with excellent biocompatibility and excellent mechanical properties. They are rich in functional groups such as aromatic rings and hydroxyl groups. These functional groups can form stable chemical bonds with metal surfaces, polymer materials, etc., to achieve good surface adhesion and lubrication effects, and have shown great application potential in the field of lubrication. However, polydopamine nanoparticles are limited by their extremely poor oil dispersion stability, which greatly limits their application as anti-friction and anti-wear additives for lubricating oils. Surface modification is one of the effective ways to solve the problem of dispersion stability of polydopamine nanoparticles in oil. However, the amino groups on the surface of polydopamine nanoparticles are relatively scarce, and the grafting density of lipophilic anions is not ideal.

[0003] Polyethyleneimine (PEI) contains a large number of amine groups, and its catechol groups can react with a variety of functional groups including amines and thiols through Michael addition or Schiff base reaction. However, the two-step grafting method is difficult to operate, and the high charge density of PEI will cause polydopamine nanoparticles to precipitate due to charge effects. Therefore, the development of a simple and efficient modification synthesis method is of great significance for the design and preparation of oil-soluble organic polymer nanoparticles and their application as oil-based lubricant additives. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a polyelectrolyte hybrid polydopamine nanoparticle and a preparation method and application thereof, so as to solve the technical problem of poor stability of polydopamine type lubricating oil additives.

[0005] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing polyelectrolyte hybrid polydopamine nanoparticles, comprising the following steps:

[0006] S1. Dissolve polyethyleneimine (PEI) and dopamine hydrochloride separately, then mix the solutions, stir and react at 25-35° C. for 12-24 hours, and then centrifuge to obtain polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs); the mass ratio of polyethyleneimine to dopamine hydrochloride is 1-3:10-20;

[0007] Polyethyleneimine (PEI) has a large number of amine groups. The introduction of polyethyleneimine can make the surface of polydopamine nanoparticles have more reactive sites, thereby increasing the grafting rate of oil-soluble anions. At the same time, PEI can provide an alkaline environment for dopamine polymerization. Among them, the amount of PEI should not be too much or too little. When the PEI concentration in the reaction system is too high, the adhesion between the nanoparticles will increase and agglomeration will occur, affecting the water dispersion ability of the nanoparticles; when the amount of PEI is too little, there will be too few PEI chains on the surface of the particles, which is not conducive to subsequent modification. If too much dopamine hydrochloride is added, the size of the polymerized polydopamine nanoparticles will become larger and it will be difficult to achieve the expected effect; if too little dopamine hydrochloride is added, it will be difficult to polymerize into polydopamine nanoparticles.

[0008] S2. Disperse polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs) in water, then adjust the pH of the dispersion to 3-4, stir for 1-2 hours to fully protonate the PEI-PDA NPs, then add a lipophilic anion salt solution, continue stirring for 0.5-1 hour, and finally centrifuge to obtain lipophilic polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs); the mass ratio of the lipophilic anion salt in the polyethyleneimine hybrid polydopamine nanoparticles and the lipophilic anion salt solution is 1:1-3.

[0009] On the basis of the above technical solution, the present invention can also be improved as follows:

[0010] Furthermore, the relative molecular mass of polyethyleneimine is 600 (PEI 600 )、1000(PEI 1000 ) and 1800(PEI 1800 ).

[0011] Furthermore, the reaction temperature in S1 is 30° C. and the reaction time is 18 h.

[0012] Furthermore, the centrifugal speed in S1 is 11000-12000 r / min, and the centrifugal time is 20-30 min; the centrifugal speed in S2 is 3600-4000 r / min, and the centrifugal time is 3-6 min.

[0013] When collecting and purifying PEI-PDA NPs in S1, the reaction solution is centrifuged at 11000-12000 r / min for 20-30 min to collect PEI-PDA NPs. If the speed is too low and the time is too short, too many nanoparticles will remain in the supernatant and cause waste; if the speed is too high and the time is too long, it will be detrimental to the subsequent dispersion of the nanoparticles in water.

[0014] Furthermore, after centrifugation in S1 and S2, the solid particles are washed 3-5 times to remove the residual ethanol in the particles and the PEI that is not firmly grafted on the particle surface.

[0015] Furthermore, when collecting and purifying PEI-PDA NPs, an organic solvent sedimentation method can also be used for collection.

[0016] Furthermore, the reagent used to adjust the dispersion is hydrochloric acid, hydrofluoric acid or acetic acid.

[0017] Furthermore, the concentration of the reagent used to adjust the dispersion is 0.05-0.2 mol / L.

[0018] The concentration of the reagent used to adjust the dispersion should not be too high, as too high a concentration will cause the PEI-PDA NPs to depolymerize, resulting in structural damage, which is not conducive to practical applications; too low a concentration will result in incomplete protonation of the nanoparticles.

[0019] Furthermore, the lipophilic anion salt solution is a lithium disalicylate borate (Li-BScB) solution or a sodium oleate (Na-OL) solution.

[0020] Furthermore, the concentration of the lipophilic anion salt solution is 0.05-0.1 mol / L.

[0021] Furthermore, after washing the solid particles obtained by centrifugation, S2 also includes uniformly dispersing the solid particles in a polar solvent, and then ventilating at 25-45° C. for 6-8 hours to obtain polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDANPs).

[0022] If the precipitate obtained by centrifugation of S2 is directly dried, the LPEI-PDA NPs deposited together will cause the adhesion between particles, affecting the oil dispersibility of LPEI-PDA NPs, so the present invention uses a volatile polar solvent to disperse the LPEI-PDA NPs deposited together, and then the polar solvent is dried at low temperature to obtain LPEI-PDA NPs. Since polyethylene glycol (PEG) itself belongs to polar base oil, ethyl acetate or anhydrous ethanol can be selected as the polar solvent with a low boiling point here. For the removal of polar solvents, generally vacuum distillation, natural volatilization or rotary evaporation can be used, but the removal efficiency of natural volatilization is too low, and the removal methods with high efficiency such as vacuum distillation and rotary evaporation will increase the difficulty of collecting the product. Therefore, the present invention removes polar solvents under ventilation conditions of 25-45°C, which will not affect the structure and performance of LPEI-PDA NPs, and can ensure that the solvent is removed at a faster speed under ventilation conditions at the same time.

[0023] The invention also discloses polyelectrolyte hybrid polydopamine nanoparticles prepared by the preparation method.

[0024] The invention also discloses the application of polyelectrolyte hybrid polydopamine nanoparticles in the preparation of lubricating oil additives.

[0025] Furthermore, the addition amount of the polyelectrolyte hybrid polydopamine nanoparticles is 1-7 wt % of the lubricating oil base oil.

[0026] Furthermore, the lubricating oil base oil is polyethylene glycol (PEG).

[0027] The beneficial effects of the present invention are as follows: the present invention adopts a one-pot method to prepare polyethyleneimine-modified polydopamine nanoparticles, thereby avoiding the occurrence of coagulation due to the strong charge interaction between polydopamine nanoparticles and polyethyleneimine in the two-step grafting. During the preparation process, PEI provides an alkaline environment for the polymerization of dopamine and plays the role of a surface modifier. The successful modification of PEI increases the amino groups on the surface of the polydopamine nanoparticles, provides more active sites that can be protonated, thereby effectively improving the grafting rate of lipophilic anions on the surface of the polydopamine nanoparticles. A higher grafting density of lipophilic anions is conducive to the stable dispersion of nanoparticles in polyethylene glycol base oil. In addition, polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs) with rich anionic groups can achieve rapid adsorption on the surface of steel sheets through electrostatic action, thereby promoting the formation of a physical adsorption film. The method of the present invention is simple and easy to operate, and avoids the nearly harsh condition control in the two-step grafting. At the same time, the post-processing steps are reduced by centrifuging the LPEI-PDA NPs and dissolving and purifying them with anhydrous ethanol, thereby greatly improving the preparation efficiency of the LPEI-PDA NPs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the SEM morphology of PEI-PDA NPs prepared in comparative example;

[0029] Figure 2 This is the SEM morphology of LPEI-PDANPs prepared in Example 1;

[0030] Figure 3 XPS graphs of PEI-PDANPs and LPEI-PDA NPs;

[0031] Figure 4 Comparison of the stability of PEI-PDANPs and LPEI-PDANPs;

[0032] Figure 5 Comparison of the friction reducing properties of LPEI-PDA NPs prepared in Examples 1-3;

[0033] Figure 6 The effect of the addition amount of LPEI-PDANPs on the anti-wear performance;

[0034] Figure 7 is the cross-sectional view of the wear track of the base oil without adding LPEI-PDANPs;

[0035] Figure 8 2D image of the wear track of the base oil without LPEI-PDANPs added;

[0036] Fig. 9 3D image of the wear track of the base oil without LPEI-PDANPs added;

[0037] Fig.10 Cross-sectional view of the wear track of the base oil with 5 wt% LPEI-PDANPs added;

[0038] Fig.11 2D image of the wear track of the base oil with 5 wt% LPEI-PDA NPs added;

[0039] Fig.12 3D image of the wear track of the base oil with 5 wt% LPEI-PDANPs added. DETAILED DESCRIPTION

[0040] The specific embodiments of the present invention are described below to facilitate the understanding of the present invention by those skilled in the art. If the specific conditions are not specified in the examples, the methods are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. However, it should be clear that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

[0041] Example 1

[0042] A method for preparing polyelectrolyte hybrid polydopamine nanoparticles comprises the following steps:

[0043] S1, 0.1g polyethyleneimine (PEI 600 ) was dissolved in an ethanol solution (80 mL water + 40 mL ethanol), stirred in a 30°C water bath for 30 min, 0.5 g dopamine hydrochloride was dissolved in 10 mL water, and then the dopamine hydrochloride solution was added dropwise to the polyethyleneimine solution, stirred at 30°C for 18 h, and then the black solution after the reaction was centrifuged at 11500 r / min for 25 min to obtain a precipitate, and the precipitate was washed 4 times with deionized water to obtain polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDANPs);

[0044] S2. Disperse 0.1 g of polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDANPs) in 20 mL of water, then adjust the pH of the dispersion to 3.5 with 0.1 mol / L hydrochloric acid, stir for 1.5 h to fully protonate the PEI-PDANPs, then add 10 mL of 0.1 mol / L lithium disalicylate borate (Li-BScB) solution, continue stirring for 1 h, then centrifuge the reaction suspension at 3800 r / min for 5 min, wash the obtained solid particles 4 times, and finally evenly disperse the solid particles in anhydrous ethanol, then ventilate at 30 ° C for 7 h to remove the anhydrous ethanol to obtain polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDANPs).

[0045] Example 2

[0046] A method for preparing polyelectrolyte hybrid polydopamine nanoparticles comprises the following steps:

[0047] S1, 0.15g polyethyleneimine (PEI 1000 ) was dissolved in an ethanol solution (80 mL water + 40 mL ethanol), stirred in a water bath at 30°C for 25 min, 0.5 g dopamine hydrochloride was dissolved in 10 mL water, and then the dopamine hydrochloride solution was added dropwise to the polyethyleneimine solution, stirred at 35°C for 12 h, and then the black solution after the reaction was centrifuged at 11000 r / min for 30 min to obtain a precipitate, and the precipitate was washed with deionized water 5 times to obtain polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDANPs);

[0048] S2. Disperse 0.1 g of polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs) in 20 mL of water, then adjust the pH of the dispersion to 3 with 0.15 mol / L hydrofluoric acid, stir for 1 h to fully protonate the PEI-PDA NPs, then add 10 mL of 0.1 mol / L sodium oleate (Na-OL) solution, continue stirring for 0.5 h, then centrifuge the reaction suspension at 4000 r / min for 3 min, wash the obtained solid particles 3 times, and finally evenly disperse the solid particles in ethyl acetate, then ventilate at 45 ° C for 6 h to remove ethyl acetate to obtain polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs).

[0049] Example 3

[0050] A method for preparing polyelectrolyte hybrid polydopamine nanoparticles comprises the following steps:

[0051] S1, 0.05g polyethyleneimine (PEI 1800) was dissolved in an ethanol solution (80 mL water + 40 mL ethanol), stirred in a 30°C water bath for 30 min, 1 g dopamine hydrochloride was dissolved in 10 mL water, and then the dopamine hydrochloride solution was added dropwise to the polyethyleneimine solution, stirred at 25°C for 24 h, and then the black solution after the reaction was centrifuged at 12000 r / min for 20 min to obtain a precipitate, and the precipitate was washed 3 times with deionized water to obtain polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDANPs);

[0052] S2. Disperse 0.2 g of polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs) in 20 mL of water, then adjust the pH of the dispersion to 4 with 0.1 mol / L acetic acid, stir for 2 h to fully protonate the PEI-PDA NPs, then add 10 mL of 0.1 mol / L lithium disalicylate borate (Li-BScB) solution, continue stirring for 1 h, then centrifuge the reaction suspension at 3600 r / min for 6 min, wash the obtained solid particles 5 times, and finally evenly disperse the solid particles in anhydrous ethanol, then ventilate at 25 ° C for 8 h to remove the anhydrous ethanol to obtain polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs).

[0053] Comparative Example

[0054] The difference between this comparative example and Example 1 is that step S2 is omitted to prepare polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs).

[0055] Experimental example

[0056] 1. SEM analysis

[0057] The products of the comparative example and embodiment 1 were subjected to SEM analysis, and the results were as follows: Figure 1-Figure 2 As shown. Figure 1 The SEM morphology of polyethyleneimine hybrid polydopamine nanoparticles (PEI-PDA NPs) prepared in the comparative example is shown in FIG. Figure 2 The SEM morphology of the polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs) prepared in Example 1. It can be seen from the figure that the average particle size of the PEI-PDA NPs before modification is 41.64nm and the shape is spherical; after modification, the particles of the LPEI-PDA NPs still maintain a spherical structure with an average particle size of 43.13nm, indicating that the modification process did not significantly destroy the morphology of the polydopamine nanoparticles. The increase in particle size also shows that BScB – Successful retention on the surface of polydopamine nanoparticles.

[0058] 2.XPS analysis

[0059] The products of the comparative example and embodiment 1 were subjected to XPS analysis, and the results were as follows: Figure 3 As shown in the figure, compared with the unmodified PEI-PDANPs, the modified LPEI-PDANPs are richer in elements. In addition to C, N and O elements, more BScB - The corresponding signal of the B element was detected, and the Cl element was not detected in the modified sample, indicating that the ion exchange was relatively thorough.

[0060] 3. Stability test

[0061] The compatibility with lubricating oil is one of the important criteria for measuring whether nanoparticles can be used as lubricating additives. Take the products of the comparative example and Example 1, add them to the polyethylene glycol 200 base oil at an addition amount of 2wt%, and then let it stand for a period of time to test its stability. The results are as follows Figure 4 As shown, the LPEI-PDA NPs prepared in Example 1 had no obvious precipitation after being added to the base oil for thirty days, showing good dispersion stability. However, the polyethyleneimine-modified polydopamine nanoparticles prepared in the comparative example before modification were difficult to disperse in the oil and obviously precipitated on the second day.

[0062] 4. Wear resistance test

[0063] like Figure 5 As shown, when the addition amount of LPEI-PDA NPs is 5wt%, the friction reducing performance of LPEI-PDA NPs prepared in Example 1 is the best.

[0064] The polyelectrolyte hybrid polydopamine nanoparticles (LPEI-PDA NPs) prepared in Example 1 were added to the base oil in different amounts (0-7wt%), and the lubrication performance of the steel / steel friction pair was tested under the conditions of a load of 30N, a speed of 2cm / s, and a friction time of 30min. The results are as follows: Figure 6 As shown in the figure, it can be seen that the use of the LPEI-PDANPs prepared in the present invention as a lubricant additive can significantly improve the lubrication performance of the base oil, wherein when the addition amount is 5wt%, the friction reduction performance of the lubricant is the best.

[0065] At the same time, the wear scars of lubricating oils without and with 5 wt% LPEI-PDA NPs were scanned under a 3D profilometer. By comparing the cross-section, 2D and 3D images of the wear tracks of the two, it was found that the addition of LPEI-PDA NPs can effectively improve the anti-wear properties of the base oil ( Figure 7-Figure 12 ).

Claims

1. A method for preparing polyelectrolyte hybrid polydopamine nanoparticles, It is characterized in that The following steps are involved: S1. Dissolve polyethyleneimine and dopamine hydrochloride separately, then mix the solutions, stir and react at 25-35° C. for 12-24 hours, and then centrifuge to obtain polyethyleneimine hybrid polydopamine nanoparticles; the mass ratio of polyethyleneimine to dopamine hydrochloride is 1-3:10-20; S2. Dispersing polyethyleneimine hybrid polydopamine nanoparticles in water, then adjusting the pH of the dispersion to 3-4, adding a lipophilic anion salt solution after stirring for 1-2 hours, continuing to stir for 0.5-1 hour, and finally centrifuging to obtain lipophilic polyelectrolyte hybrid polydopamine nanoparticles; the mass ratio of the polyethyleneimine hybrid polydopamine nanoparticles to the lipophilic anion salt in the lipophilic anion salt solution is 1:1-3.

2. The method for preparing polyelectrolyte hybrid polydopamine nanoparticles according to claim 1, It is characterized in that The reaction temperature in S1 is 30° C. and the reaction time is 18 h.

3. The method for preparing polyelectrolyte hybrid polydopamine nanoparticles according to claim 1, It is characterized in that The centrifugal speed in S1 is 11000-12000 r / min, and the centrifugal time is 20-30 min; the centrifugal speed in S2 is 3600-4000 r / min, and the centrifugal time is 3-6 min.

4. The method for preparing polyelectrolyte hybrid polydopamine nanoparticles according to claim 1, It is characterized in that The reagent used for adjusting the dispersion is hydrochloric acid, hydrofluoric acid or acetic acid.

5. The method for preparing polyelectrolyte hybrid polydopamine nanoparticles according to claim 1, It is characterized in that The lipophilic anion salt solution is a lithium borate disalicylate solution or a sodium oleate solution.

6. The method for preparing the polyelectrolyte hybrid polydopamine nanoparticles according to claim 1 or 5, It is characterized in that The concentration of the lipophilic anion salt solution is 0.05-0.1 mol / L.

7. A polyelectrolyte hybrid polydopamine nanoparticle, It is characterized in that The nanoparticles are prepared by the method for preparing the polyelectrolyte hybrid polydopamine nanoparticles according to any one of claims 1 to 6.

8. Use of the polyelectrolyte hybrid polydopamine nanoparticles according to claim 7 in the preparation of lubricating oil additives.

9. The use according to claim 8, It is characterized in that The addition amount of the polyelectrolyte hybrid polydopamine nanoparticles is 1-7wt% of the lubricating oil base oil.

10. The use according to claim 9, It is characterized in that The lubricating oil base oil is polyethylene glycol.