Industrial anti-aging rubber compound and preparation method thereof

By using aging-resistant kneaded glue composed of methylphenylethylene silicone rubber and nanofillers, the aging problem of industrial kneaded glue in complex environments is solved, and its tensile strength, wear resistance and aging resistance are improved. Extend service life.

CN118895051AInactive Publication Date: 2024-11-05WENZHOU HEFENG SILICONE RUBBER IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411087706.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing industrial mixed glues are prone to aging in complex environments such as high temperature, high humidity, and chemical corrosion, resulting in unstable performance, insufficient tensile strength, wear resistance and chemical corrosion resistance, which affects service life and reliability.

Method used

Aging-resistant kneaded glue composed of methylphenylethylene silicone rubber, nanofillers, phenolamine organic compounds and vulcanizing agents is enhanced through specific preparation methods and process flows. .

Benefits of technology

It significantly improves the tensile strength, wear resistance and aging resistance of the mixed glue, extends the service life, and enhances the performance stability under different environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985634990000071
    Figure BDA0004985634990000071
  • Figure BDA0004985634990000072
    Figure BDA0004985634990000072
  • Figure BDA0004985634990000081
    Figure BDA0004985634990000081
Patent Text Reader

Abstract

The invention provides an industrial anti-aging rubber compound and a preparation method thereof, and the industrial anti-aging rubber compound comprises the following components in parts by weight: 60-80 parts of methyl phenyl vinyl silicone rubber, 20-35 parts of a nano filler, 8-12 parts of a phenol amine organic matter, 2-5 parts of a vulcanizing agent and 1-2.5 parts of a flame retardant, the industrial anti-aging rubber compound has the advantages of excellent tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicone rubber, and in particular to an industrial aging-resistant mixed rubber and a preparation method thereof. Background Art

[0002] Rubber mix refers to a rubber compound made by mixing rubber and various compounding agents. According to the type of rubber, there are natural rubber mix and synthetic rubber mix (such as styrene-butadiene rubber, butadiene rubber, etc.). According to the application field, there are automotive mix, electronic mix, aerospace mix, etc. The development of industrial rubber mix began in the late 19th century and early 20th century. At that time, natural rubber was mainly used as a raw material, and the types and applications of compounding agents were relatively simple. With the progress of the chemical industry, synthetic rubber has gradually emerged, and its performance has been continuously optimized. Together with natural rubber mix, it has met the growing demand in the industrial field. In recent years, with the rapid development of science and technology, industrial rubber mix has made significant progress in performance, quality and application fields. New compounding agents, advanced mixing processes and high-performance rubber materials have continued to emerge, which has greatly improved the aging resistance of rubber mixes.

[0003] In many industrial application scenarios, such as high temperature, high humidity, strong chemical corrosion, etc., the aging resistance of rubber compounds is severely challenged. In order to reduce maintenance costs and improve production efficiency, industrial products need to have longer service life and higher reliability, which requires rubber compounds to have excellent aging resistance. The increasingly stringent environmental regulations and the continuous improvement of industry standards have prompted companies to develop and use more aging-resistant rubber compounds to reduce the impact on the environment and meet market access requirements. Improvement of rubber materials: Develop new rubber varieties, such as special rubbers with excellent aging resistance. Modify the molecular structure of traditional rubber to improve its antioxidant and thermal oxidative aging resistance. Optimization of compounding agents: The development and application of antioxidants, anti-ozonants, etc. effectively delay the aging process of rubber. The emergence of new functional compounding agents, such as ultraviolet absorbers and light stabilizers, further enhances the aging resistance of rubber compounds. Innovation of mixing process: Use advanced mixing equipment and processes, such as internal mixers and continuous mixing technology, to improve the uniformity and stability of rubber compounds. Optimize mixing process parameters, such as temperature, time, speed, etc., to improve the performance of the mixed rubber. Improvement of aging performance evaluation methods: Establish more accurate and comprehensive aging performance test standards and methods, such as accelerated aging tests, natural aging tests, etc. Use advanced analytical testing technologies, such as infrared spectroscopy and thermal analysis, to conduct in-depth research on chemical changes and microstructural evolution during the aging process.

[0004] In current industrial applications, the performance of rubber compounds faces a series of challenges and shortcomings:

[0005] First, the limitation of aging resistance. Despite continuous improvement measures, the rubber compound may still age under long-term exposure to complex industrial environments, such as high temperature, high humidity, strong ultraviolet rays, etc., such as hardening, brittleness, cracking, etc., thus affecting its service life and performance stability. Second, the lack of mechanical properties. For example, the tensile strength, tear strength and wear resistance of some rubber compounds may not meet the needs of some high-strength and high-wear industries. When subjected to large mechanical stress, it is easy to break or excessively wear, reducing the reliability and safety of the product. Third, the challenge of chemical corrosion resistance. In the chemical industry and other fields, rubber compounds may be exposed to various corrosive substances such as strong acids, strong alkalis, and organic solvents. However, some rubber compounds have limited corrosion resistance in these environments, and are prone to swelling, corrosion, and even decomposition, leading to problems such as seal failure and component damage. Fourth, the instability of electrical properties. For some rubber compounds used in the electronic and electrical fields, their electrical properties such as electrical insulation and conductivity may not be stable enough. Under different temperature and humidity conditions, electrical properties may change, affecting the normal operation and safety of equipment.

[0006] In summary, developing an industrial rubber compound with excellent tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and other properties is a problem to be solved urgently by the present invention. Summary of the invention

[0007] Purpose of the invention:

[0008] In view of the deficiencies in the prior art, the present invention provides an industrial anti-aging rubber compound and a preparation method thereof. The industrial anti-aging rubber compound of the present invention has excellent tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and other properties.

[0009] The technical solution of the present invention:

[0010] The invention provides an industrial anti-aging rubber compound, which is characterized in that the components of the industrial anti-aging rubber compound, measured by weight, include: 60 to 80 parts of methylphenylethylene silicone rubber, 20 to 35 parts of nanofillers, 8 to 12 parts of phenolamine organic matter, 2 to 5 parts of vulcanizing agents, and 1 to 2.5 parts of flame retardants.

[0011] Furthermore, the methylphenylvinyl silicone rubber is prepared by reacting a dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, (4-bromobenzyl)trimethylsilane, tetramethylammonium hydroxide alkali glue, and a polymerization inhibitor.

[0012] The preparation method of the methylphenylethylene silicone rubber comprises the following steps:

[0013] S1. Accurately weigh dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, (4-bromobenzyl)trimethylsilane, tetramethylammonium hydroxide alkali glue and polymerization inhibitor, and set aside;

[0014] S2, adding the methylphenylvinyl silicone rubber, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane weighed in step 1 into a reaction container, stirring and mixing at 350-400 rpm to make them evenly dispersed;

[0015] S3. After uniform dispersion, continue stirring at 350-400 rpm and gradually raise the temperature to 90-100°C. Slowly, add tetramethylammonium hydroxide alkali glue and inhibitor, and continue stirring to react for 4-6 hours.

[0016] S4. After the reaction in step 3 is completed, filtration, extraction and purification are performed to obtain methylphenylethylene silicone rubber.

[0017] Furthermore, the addition amount of the tetramethylammonium hydroxide alkali glue is 1 to 2.5% of the dimethylsiloxane mixed ring body.

[0018] Furthermore, the mass ratio of the dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane is 42-48:2-3:4-5:1.

[0019] The preparation method of the tetramethylammonium hydroxide alkali glue comprises the following steps:

[0020] S1, weigh tetramethylammonium hydroxide and hexamethylcyclotrisiloxane and put them into an alkali glue kettle with a stirring device, a vacuum system and a temperature control device, add an appropriate amount of anhydrous methanol, start stirring, the stirring speed is preferably 250-300 rpm, and gradually heat up to 60-75°C to completely dissolve tetramethylammonium hydroxide and hexamethylcyclotrisiloxane;

[0021] S2. After complete dissolution, nitrogen is continuously introduced, and the vacuum degree in the kettle is controlled to be 0.03 MPa-0.045 MPa, and then the temperature is continued to rise to 80-90°C for dehydration operation;

[0022] S3. Observe the materials in the kettle of step S3. After the mixed solution is clear and transparent, use nitrogen to eliminate the vacuum, slowly cool the alkali-gel kettle to 50-60° C., add tetramethyldivinyldisilazane, and react at normal pressure for 1.5-2 hours;

[0023] S4. After the reaction is completed, nitrogen is used to eliminate the negative pressure in the reactor to obtain tetramethylammonium hydroxide alkali glue, which is then stored under pressure, temperature and stirring conditions for later use.

[0024] Furthermore, the mass ratio of tetramethylammonium hydroxide to hexamethylcyclotrisiloxane is 1:1.5-4; and the added amount of tetramethyldivinyldisilazane is 0.5-2% of tetramethylammonium hydroxide.

[0025] Furthermore, the nano filler is a mixture of one or more of nano white carbon black, nano calcium carbonate and nano titanium dioxide.

[0026] Furthermore, the phenolamine organic matter is a mixture of one or more of p-methylphenol, N,N'-diphenyl-p-phenylenediamine, and 4-methyl-6-tert-butylphenol.

[0027] Furthermore, the vulcanizing agent is dicumyl peroxide.

[0028] Furthermore, the flame retardant is magnesium hydroxide.

[0029] The present application also provides a method for preparing an industrial aging-resistant rubber compound, comprising the following steps:

[0030] Step 1, adding methylphenylethylene silicone rubber into an internal mixer, then adding the nanofiller three times at intervals of 5 to 10 minutes, then adding phenolamine organic matter and flame retardant, continuing to internally mix for a period of time, and then cooling to room temperature to obtain a rubber preform;

[0031] Step 2: placing the preformed rubber mix in step 1 in an open mixer, adding a vulcanizing agent and vulcanizing under controlled temperature, and after the vulcanization is completed, cooling to room temperature to obtain an industrial aging-resistant rubber mix.

[0032] Furthermore, in step 1, the temperature of the internal mixer is 100-120° C., the stirring speed of the internal mixer is 300-450 rpm, and the mixing time is 10-25 minutes; in step 2, the vulcanization temperature is 160-170° C., and the vulcanization time is 0.5-1 hour.

[0033] Methylphenyl vinyl silicone rubber is a product obtained by introducing methylphenyl siloxane chain segments into the molecular chain of methylvinyl silicone rubber. In addition to the general characteristics of methylvinyl silicone rubber, it also has excellent low temperature resistance, ablation resistance and radiation resistance. By controlling the mass ratio of dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane, the prepared methylphenyl vinyl silicone rubber has excellent high and low temperature resistance and radiation resistance. When preparing tetramethylammonium hydroxide alkali rubber, the modifier tetramethyl divinyl disilazane makes the alkali rubber more soluble in siloxane. In the early polymerization stage of silicone rubber, it increases the molecular weight of the catalyst, improves the catalytic efficiency, and increases the polymerization degree of methylphenyl vinyl silicone rubber; nanofillers enhance the mechanical properties of the material, improve the strength, hardness and wear resistance, improve the thermal stability and thermal conductivity of the material, and improve the barrier properties of the material: prevent the penetration of gas and liquid; phenolamine organic matter has an antioxidant effect, delays the oxidation aging process of the material, prolongs the service life, and enhances the performance stability of the material under different environmental conditions. Vulcanizers promote rubber cross-linking, so that rubber molecules form a three-dimensional network structure, thereby improving the strength, elasticity and wear resistance of the rubber, and improving the heat resistance and aging resistance of the rubber. The vulcanized rubber has more stable performance under high temperature and long-term use conditions, so that the prepared industrial aging-resistant compound rubber has excellent tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and other properties.

[0034] Beneficial effects:

[0035] The industrial anti-aging mixed rubber of the present invention has excellent tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and other properties. DETAILED DESCRIPTION

[0036] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0037] In the following preparation examples, embodiments and comparative examples, methylphenylvinyl silicone rubber, model RS120, was purchased from Anhui Ruoshui Chemical Co., Ltd.; fluororubber was purchased from Zhejiang Jiacheng New Materials Co., Ltd.; dimethylsiloxane mixed ring body was purchased from Zhongshan Dixin Chemical Co., Ltd.; tetramethyldivinyldisiloxane was purchased from Hubei Taihechang Biotechnology Co., Ltd.; tetramethyltetravinylcyclotetrasiloxane was purchased from Zhongshan Dixin Chemical Co., Ltd.; and tetramethylammonium hydroxide was purchased from Wuhan Rongcan Biotechnology Co., Ltd.

[0038] Preparation example:

[0039] Preparation of Tetramethylammonium Hydroxide Alkaline Glue A:

[0040] S1, weigh 10g of tetramethylammonium hydroxide and 15g of hexamethylcyclotrisiloxane and put them into an alkali-gel kettle with a stirring device, a vacuum system and a temperature control device, add 1L of anhydrous methanol, start stirring, the stirring speed is 250 rpm, and gradually heat up to 75°C to completely dissolve the tetramethylammonium hydroxide and hexamethylcyclotrisiloxane;

[0041] S2. After complete dissolution, nitrogen is continuously introduced, and the vacuum degree in the kettle is controlled to 0.04 MPa, and then the temperature is continued to rise to 90°C for dehydration operation;

[0042] S3. Observe the materials in the kettle of step S3. After the mixed solution is clear and transparent, use nitrogen to eliminate the vacuum, slowly cool the alkali-gel kettle to 60° C., add 0.2 g of tetramethyldivinyldisilazane, and react at normal pressure for 2 hours;

[0043] S4. After the reaction is completed, nitrogen is used to eliminate the negative pressure in the reactor to obtain tetramethylammonium hydroxide alkali glue, which is then stored under pressure, temperature and stirring conditions for later use.

[0044] Preparation of Tetramethylammonium Hydroxide Alkaline Glue B:

[0045] The difference between this preparation and tetramethylammonium hydroxide alkali gel A is that 15 g of hexamethylcyclotrisiloxane in step S1 is replaced by 10 g of hexamethylcyclotrisiloxane.

[0046] Preparation of Tetramethylammonium Hydroxide Alkaline Glue C:

[0047] The difference between the present preparation and tetramethylammonium hydroxide alkali gel A is that 0.2 g of tetramethyldivinyldisilazane in step S3 is replaced by 0.5 g of tetramethyldivinyldisilazane.

[0048] Preparation of methylphenylethylene silicone rubber A:

[0049] S1. Accurately weigh 50 g of dimethylsiloxane mixed ring body, 2 g of tetramethyldivinyldisiloxane, 5 g of tetramethyltetravinylcyclotetrasiloxane, 1 g of (4-bromobenzyl)trimethylsilane, 0.5 g of tetramethylammonium hydroxide alkali gel A and 0.5 g of 2-tert-butylhydroquinone, and set aside;

[0050] S2, adding the methylphenylvinyl silicone rubber, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane weighed in step 1 into a reaction container, stirring and mixing at 350 rpm to make them evenly dispersed;

[0051] S3, after uniform dispersion, continue stirring at 350 rpm and gradually increase the temperature to 100°C, slowly add tetramethylammonium hydroxide alkali gel A and inhibitor, and continue stirring and reacting for 6 hours;

[0052] S4. After the reaction in step 3 is completed, filtration, extraction and purification are performed to obtain methylphenylethylene silicone rubber.

[0053] Preparation of methylphenylethylene silicone rubber B:

[0054] The difference between this preparation and methylphenylethylene silicone rubber A is that the 0.5 g of tetramethylammonium hydroxide alkali gel A weighed in step 1 is replaced by 1.25 g of tetramethylammonium hydroxide alkali gel B.

[0055] Preparation of methylphenylethylene silicone rubber C:

[0056] The difference between this preparation and methylphenylethylene silicone rubber A is that the 0.5 g of tetramethylammonium hydroxide alkali gel A weighed in step 1 is replaced by 0.5 g of tetramethylammonium hydroxide alkali gel B.

[0057] Preparation of methylphenylethylene silicone rubber D:

[0058] The difference between this preparation and methylphenylethylene silicone rubber A is that the 0.5 g of tetramethylammonium hydroxide alkali gel A weighed in step 1 is replaced by 0.5 g of tetramethylammonium hydroxide alkali gel C.

[0059] Preparation of methylphenylethylene silicone rubber E:

[0060] The difference between this preparation and methylphenylethylene silicone rubber A is that the 0.5 g of tetramethylammonium hydroxide alkali gel A weighed in step 1 is replaced by 0.25 g of tetramethylammonium hydroxide alkali gel A.

[0061] Preparation of methylphenylethylene silicone rubber F:

[0062] The difference between this preparation and methylphenylethylene silicone rubber A is that the 0.5 g of tetramethylammonium hydroxide alkali gel A weighed in step 1 is replaced by 2 g of tetramethylammonium hydroxide alkali gel A.

[0063] The method for preparing an industrial aging-resistant rubber compound comprises the following steps:

[0064] Step 1, adding methylphenylethylene silicone rubber into an internal mixer, then adding the nanofiller three times at intervals of 10 minutes, then adding phenolamine organic matter and flame retardant, and continuing to internally mix, the temperature of the internal mixer is 120° C., the stirring speed of the internal mixer is 350 rpm, the internal mixing time is 15 minutes, and then cooling to room temperature to obtain a rubber mix preform;

[0065] Step 2: Place the preformed rubber mix in step 1 in an open mixer, add a vulcanizing agent and vulcanize under controlled temperature, the vulcanization temperature is 165°C, the vulcanization time is 0.5 hours, and after the vulcanization is completed, cool to room temperature to obtain an industrial aging-resistant rubber mix.

[0066] Examples 1 to 7

[0067] According to the above-mentioned preparation method of industrial aging-resistant rubber compound, Table 1 is the ingredient list of industrial aging-resistant rubber compound of Examples 1 to 7 in parts by weight.

[0068] Table 1

[0069]

[0070] Comparative Examples 1 to 4

[0071] Comparative Examples 1 to 4 were prepared according to the above-mentioned method for preparing the industrial aging-resistant rubber compound. Table 2 is a list of ingredients in parts by weight for the preparation method of the industrial aging-resistant rubber compound of Comparative Examples 1 to 4.

[0072] Table 2

[0073]

[0074]

[0075] Performance Test:

[0076] (1) Tensile strength: Tested according to GB / T528-2009 “Vulcanized rubber or thermoplastic rubber - Determination of tensile stress-strain properties”;

[0077] (2) Wear resistance: According to GB / T 9867-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrader method)", after the test, the mass loss of the sample is measured to evaluate the wear resistance.

[0078] (3) Hot air aging test: According to GB / T 3512-2014 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber", the elongation at break of the test specimen after aging is tested.

[0079] (4) Low temperature brittleness: Tested at -80°C according to GB / T 1682-1994 “Determination of low temperature brittleness of vulcanized rubber”.

[0080] The industrial aging-resistant rubber compounds prepared in the embodiments and comparative examples were tested according to the above test method. The test results are shown in Table 1.

[0081] Table 1

[0082]

[0083]

[0084] It can be seen from Table 1 that the industrial aging-resistant rubber mixes prepared in Examples 1 to 3 have good tensile strength, wear resistance, aging resistance, high temperature and low temperature resistance and other properties; compared with Example 2, Example 4 shows that when preparing tetramethylammonium hydroxide alkali glue, the mass ratio of tetramethylammonium hydroxide and hexamethylcyclotrisiloxane is unreasonable, resulting in a lower degree of polymerization of the prepared methylvinyl silicone rubber, thereby weakening the tensile strength, wear resistance, aging resistance and high temperature resistance of the industrial aging-resistant rubber mix; Example 5 changes the amount of tetramethyldivinyldisilazane added as the modifier when preparing tetramethylammonium hydroxide alkali glue, and similarly, the tensile strength, wear resistance, aging resistance and high temperature resistance of the prepared industrial aging-resistant rubber mix are weakened; compared with Example 2, Example 6 to 7 shows that when preparing methylphenylvinyl silicone rubber, tetramethylammonium hydroxide alkali Unreasonable rubber dosage will lead to the deterioration of the tensile strength, wear resistance, aging resistance and high temperature resistance of the prepared industrial aging-resistant rubber compound; from comparative examples 1 to 2, it can be seen that when the amount of methylphenylethylene silicone rubber is too much or too little, the tensile strength, wear resistance, aging resistance and high temperature resistance of the prepared industrial aging-resistant rubber compound deteriorate and fail to achieve the expected effect; from comparative example 3, it can be seen that the tensile strength, wear resistance, aging resistance and high temperature and low temperature resistance of the prepared industrial aging-resistant rubber compound are not good when the methylphenylethylene silicone rubber is replaced with fluororubber on the market; from comparative example 4, it can be seen that the tensile strength, wear resistance, aging resistance and high temperature and low temperature resistance of the prepared industrial aging-resistant rubber compound are not as good as the methylphenylethylene silicone rubber prepared by the present invention when the methylphenylethylene silicone rubber is replaced with methylphenylethylene silicone rubber RS120 sold on the market.

[0085] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An industrial anti-aging rubber compound, characterized in that: The components of the industrial anti-aging rubber compound include, by weight: 60 to 80 parts of methylphenylethylene silicone rubber, 20 to 35 parts of nano fillers, 8 to 12 parts of phenolamine organic matter, 2 to 5 parts of vulcanizing agent, and 1 to 2.5 parts of flame retardant.

2. An industrial aging-resistant rubber compound according to claim 1, characterized in that: The methylphenylvinyl silicone rubber is prepared by reacting a dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, (4-bromobenzyl)trimethylsilane, tetramethylammonium hydroxide alkali glue and a polymerization inhibitor.

3. An industrial aging-resistant rubber compound according to claim 1, characterized in that: The preparation method of the methylphenylethylene silicone rubber comprises the following steps: S1. Accurately weigh dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, (4-bromobenzyl)trimethylsilane, tetramethylammonium hydroxide alkali glue and polymerization inhibitor, and set aside; S2, adding the methylphenylvinyl silicone rubber, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane weighed in step 1 into a reaction container, stirring and mixing at 350-400 rpm to make them evenly dispersed; S3. After uniform dispersion, continue stirring at 350-400 rpm and gradually raise the temperature to 90-100°C. Slowly, add tetramethylammonium hydroxide alkali glue and inhibitor, and continue stirring to react for 4-6 hours. S4. After the reaction in step 3 is completed, filtration, extraction and purification are performed to obtain methylphenylethylene silicone rubber.

4. An industrial aging-resistant rubber compound according to claim 3, characterized in that: The added amount of the tetramethylammonium hydroxide alkali glue is 1-2.5% of the dimethylsiloxane mixed ring body.

5. An industrial aging-resistant rubber compound according to claim 3, characterized in that: The mass ratio of the dimethylsiloxane mixed ring body, tetramethyldivinyldisiloxane, tetramethyltetravinylcyclotetrasiloxane and (4-bromobenzyl)trimethylsilane is 42-48:2-3:4-5:

1.

6. An industrial aging-resistant rubber compound according to claim 4, characterized in that: The preparation method of the tetramethylammonium hydroxide alkali glue comprises the following steps: S1. Weigh tetramethylammonium hydroxide and hexamethylcyclotrisiloxane and put them into an alkali-gel kettle with a stirring device, a vacuum system and a temperature control device, add an appropriate amount of anhydrous methanol, start stirring, the stirring speed is 250-300 rpm, and gradually heat up to 60-75° C. to completely dissolve tetramethylammonium hydroxide and hexamethylcyclotrisiloxane; S2. After complete dissolution, nitrogen is continuously introduced, and the vacuum degree in the kettle is controlled to be 0.03 MPa-0.045 MPa, and then the temperature is continued to rise to 80-90°C for dehydration operation; S3. Observe the materials in the kettle of step S3. After the mixed solution is clear and transparent, use nitrogen to eliminate the vacuum, slowly cool the alkali-gel kettle to 50-60° C., add tetramethyldivinyldisilazane, and react at normal pressure for 1.5-2 hours; S4. After the reaction is completed, nitrogen is used to eliminate the negative pressure in the reactor to obtain tetramethylammonium hydroxide alkali glue, which is then stored under pressure, temperature and stirring conditions for later use.

7. An industrial aging-resistant rubber compound according to claim 6, characterized in that: The mass ratio of tetramethylammonium hydroxide to hexamethylcyclotrisiloxane is 1:1.5-4; the added amount of tetramethyldivinyldisilazane is 0.5-2% of tetramethylammonium hydroxide.

8. An industrial aging-resistant rubber compound according to claim 1, characterized in that: The nano filler is a mixture of one or more of nano white carbon black, nano calcium carbonate and nano titanium dioxide; the phenolamine organic matter is a mixture of one or more of p-methylphenol, N,N'-diphenyl p-phenylenediamine and 4-methyl-6-tert-butylphenol.

9. A method for preparing the industrial aging-resistant rubber compound according to any one of claims 1 to 8, comprising the following steps: Step 1, adding methylphenylethylene silicone rubber into an internal mixer, then adding the nanofiller three times at intervals of 5 to 10 minutes, then adding phenolamine organic matter and flame retardant, continuing to internally mix for a period of time, and then cooling to room temperature to obtain a rubber preform; Step 2: placing the preformed rubber mix in step 1 in an open mixer, adding a vulcanizing agent and vulcanizing under controlled temperature, and after the vulcanization is completed, cooling to room temperature to obtain an industrial aging-resistant rubber mix.

10. The method for preparing an industrial aging-resistant rubber compound according to claim 9, characterized in that: In the first step, the temperature of the internal mixer is 100-120° C., the stirring speed of the internal mixer is 300-450 rpm, and the mixing time is 10-25 minutes; in the second step, the vulcanization temperature is 160-170° C., and the vulcanization time is 0.5-1 hour.

Citation Information

Patent Citations

  • Preparation method of methyl phenyl vinyl silicone oil

    CN103012797A

  • Preparation method for methyl vinyl silicone rubber

    CN105237769A

  • Method for producing methyl vinyl silicone rubber by continuous process

    CN110437450A

  • Polysiloxane composition with high weather resistance for external insulation and preparation method thereof

    CN117186649A

  • High-performance alkali glue and preparation method thereof

    CN117603451A